EN 573-3 Grade AW-5019 O3

Want to keep this datasheet? Save it now in your required format

Related Standards

Equivalent Materials

This material data has been provided by AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyValueConditionRelated StandardsShape

Density

2.64 g/cm³

Show Material materials with Density of 2.64 g/cm³

O3

EN 573-3, EN 1715-3

Rod, Tube, Wire

Mechanical

PropertyValueConditionRelated StandardsShapeComment

Elastic modulus

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

O3

EN 573-3, EN 1715-3

Rod, Tube, Wire

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 5000 Series Aluminium

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 5000 Series Aluminium

Shear modulus

26.0 - 26.5 GPa

Show Material materials with Shear modulus of 26.0 - 26.5 GPa

Typical for Wrought 5000 Series Aluminium

Tensile strength

250.0 - 310.0 MPa

Show Material materials with Tensile strength of 250.0 - 310.0 MPa

O3

EN 573-3, EN 1715-3

Rod, Tube, Wire

Thermal

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coefficient of thermal expansion

300 °C, 20 °C

2.61e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.61e-05 1/K

O3

EN 573-3, EN 1715-3

Rod, Tube, Wire

200 °C, 20 °C

2.51e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.51e-05 1/K

O3

EN 573-3, EN 1715-3

Rod, Tube, Wire

100 °C, 20 °C

2.41e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.41e-05 1/K

O3

EN 573-3, EN 1715-3

Rod, Tube, Wire

20 °C, -50 °C

2.2499999999999998e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.2499999999999998e-05 1/K

O3

EN 573-3, EN 1715-3

Rod, Tube, Wire

Max service temperature

150.0 °C

Show Material materials with Max service temperature of 150.0 °C

Typical for Wrought 5000 Series Aluminium

Melting point

575.0 - 630.0 °C

Show Material materials with Melting point of 575.0 - 630.0 °C

O3

EN 573-3, EN 1715-3

Rod, Tube, Wire

Specific heat capacity

904.0 J/(kg·K)

Show Material materials with Specific heat capacity of 904.0 J/(kg·K)

O3

EN 573-3, EN 1715-3

Rod, Tube, Wire

Thermal conductivity

110.0 - 140.0 W/(m·K)

Show Material materials with Thermal conductivity of 110.0 - 140.0 W/(m·K)

O3

EN 573-3, EN 1715-3

Rod, Tube, Wire

Electrical

PropertyValueConditionRelated StandardsShape

Electrical conductivity

15000000.0 - 19000000.0 S/m

Show Material materials with Electrical conductivity of 15000000.0 - 19000000.0 S/m

O3

EN 573-3, EN 1715-3

Rod, Tube, Wire

Electrical resistivity

5.26e-08 - 6.67e-08 Ω·m

Show Material materials with Electrical resistivity of 5.26e-08 - 6.67e-08 Ω·m

O3

EN 573-3, EN 1715-3

Rod, Tube, Wire

Chemical properties

PropertyValueConditionRelated StandardsShape

Chromium

0.2 %

Show Material materials with Chromium of 0.2 %

O3

EN 573-3, EN 1715-3

Rod, Tube, Wire

Copper

0.1 %

Show Material materials with Copper of 0.1 %

O3

EN 573-3, EN 1715-3

Rod, Tube, Wire

Iron

0.50 %

Show Material materials with Iron of 0.50 %

O3

EN 573-3, EN 1715-3

Rod, Tube, Wire

Magnesium

4.5 - 5.6 %

Show Material materials with Magnesium of 4.5 - 5.6 %

O3

EN 573-3, EN 1715-3

Rod, Tube, Wire

Manganese

0.1 - 0.6 %

Show Material materials with Manganese of 0.1 - 0.6 %

O3

EN 573-3, EN 1715-3

Rod, Tube, Wire

Silicon

0.4 %

Show Material materials with Silicon of 0.4 %

O3

EN 573-3, EN 1715-3

Rod, Tube, Wire

Titanium

0.2 %

Show Material materials with Titanium of 0.2 %

O3

EN 573-3, EN 1715-3

Rod, Tube, Wire

Zinc

0.2 %

Show Material materials with Zinc of 0.2 %

O3

EN 573-3, EN 1715-3

Rod, Tube, Wire

Technological properties

Property
Anodizing

decorative: sufficient, Protective: very good

Brazing

hard brazing (with flux/ without flux): poor / poor, friction soldering: acceptable, soft brazing with flux: poor

Corrosion properties

Seawater: very good, weathering: very good

Workability

Bending / Spinning (cold): good / sufficient, Impact extrusion (cold): poor, Deep drawing / upsetting (Condition) good (O) / good (O)