EN 573-3 Grade 3.4365 T73511

Want to keep this datasheet? Save it now in your required format

Description

DIN 3.4365 is a high-strength alloy that offers good stress-corrosion cracking resistance. Known as a mainstay in the aerospace industry since it was introduced, Aluminum 7075 brings moderate toughness as well as an excellent strength-to-weight ratio. It is also important to note that at sub-zero temperatures Aluminum 7075 increases in strength.

Related Standards

Equivalent Materials

This material data has been provided by AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyValueConditionRelated Standards

Density

2.8 g/cm³

Show Material materials with Density of 2.8 g/cm³

T73511

EN 573-3, EN 754, EN 755

Mechanical

PropertyValueConditionRelated StandardsComment

Elastic modulus

72.0 GPa

Show Material materials with Elastic modulus of 72.0 GPa

T73511

EN 573-3, EN 754, EN 755

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 7000 Series Aluminium

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 7000 Series Aluminium

Shear modulus

27.1 GPa

Show Material materials with Shear modulus of 27.1 GPa

T73511

EN 573-3, EN 754, EN 755

Tensile strength

440.0 MPa

Show Material materials with Tensile strength of 440.0 MPa

T73511

EN 573-3, EN 755

455.0 MPa

Show Material materials with Tensile strength of 455.0 MPa

T73511

EN 573-3, EN 754

470.0 MPa

Show Material materials with Tensile strength of 470.0 MPa

T73511

EN 573-3, EN 755

475.0 MPa

Show Material materials with Tensile strength of 475.0 MPa

T73511

EN 573-3, EN 755

485.0 MPa

Show Material materials with Tensile strength of 485.0 MPa

T73511

EN 573-3, EN 755

Thermal

PropertyTemperatureValueConditionRelated Standards

Coefficient of thermal expansion

-50 °C

2.16e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.16e-05 1/K

T73511

EN 573-3, EN 754, EN 755

20 °C

2.16e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.16e-05 1/K

T73511

EN 573-3, EN 754, EN 755

20 °C

2.3399999999999996e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3399999999999996e-05 1/K

T73511

EN 573-3, EN 754, EN 755

20 °C

2.43e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.43e-05 1/K

T73511

EN 573-3, EN 754, EN 755

20 °C

2.52e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.52e-05 1/K

T73511

EN 573-3, EN 754, EN 755

100 °C

2.3399999999999996e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3399999999999996e-05 1/K

T73511

EN 573-3, EN 754, EN 755

200 °C

2.43e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.43e-05 1/K

T73511

EN 573-3, EN 754, EN 755

300 °C

2.52e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.52e-05 1/K

T73511

EN 573-3, EN 754, EN 755

Melting point

480.0 - 640.0 °C

Show Material materials with Melting point of 480.0 - 640.0 °C

T73511

EN 573-3, EN 754, EN 755

Specific heat capacity

862.0 J/(kg·K)

Show Material materials with Specific heat capacity of 862.0 J/(kg·K)

T73511

EN 573-3, EN 754, EN 755

Thermal conductivity

130.0 - 160.0 W/(m·K)

Show Material materials with Thermal conductivity of 130.0 - 160.0 W/(m·K)

T73511

EN 573-3, EN 754, EN 755

Electrical

PropertyValueConditionRelated Standards

Electrical conductivity

19000000.0 - 23000000.0 S/m

Show Material materials with Electrical conductivity of 19000000.0 - 23000000.0 S/m

T73511

EN 573-3, EN 754, EN 755

Electrical resistivity

4.35e-08 - 5.26e-08 Ω·m

Show Material materials with Electrical resistivity of 4.35e-08 - 5.26e-08 Ω·m

T73511

EN 573-3, EN 754, EN 755

Chemical properties

PropertyValueConditionRelated Standards

Chromium

0.18 - 0.28 %

Show Material materials with Chromium of 0.18 - 0.28 %

T73511

EN 573-3, EN 754, EN 755

Copper

1.2 - 2.0 %

Show Material materials with Copper of 1.2 - 2.0 %

T73511

EN 573-3, EN 754, EN 755

Iron

0.50 %

Show Material materials with Iron of 0.50 %

T73511

EN 573-3, EN 754, EN 755

Magnesium

2.1 - 2.9 %

Show Material materials with Magnesium of 2.1 - 2.9 %

T73511

EN 573-3, EN 754, EN 755

Manganese

0.3 %

Show Material materials with Manganese of 0.3 %

T73511

EN 573-3, EN 754, EN 755

Silicon

0.4 %

Show Material materials with Silicon of 0.4 %

T73511

EN 573-3, EN 754, EN 755

Titanium

0.2 %

Show Material materials with Titanium of 0.2 %

T73511

EN 573-3, EN 754, EN 755

Zinc

5.1 - 6.1 %

Show Material materials with Zinc of 5.1 - 6.1 %

T73511

EN 573-3, EN 754, EN 755

Technological properties

Property
Anodizing

decorative: not suitable, Protective: acceptable

Brazing

hard brazing (with flux/ without flux): not suitable / not suitable, friction soldering: not suitable, soft brazing with flux: not suitable

Corrosion properties

Seawater: sufficient to poor, weathering: sufficient to poor

Workability

Bending / Spinning (cold): sufficient (O) / not suitable, Impact extrusion (cold): not suitable, Deep drawing / upsetting (Condition) not suitable / not suitable