The material: 'Kynar Flex® 2800-00' you were looking for has been superseded by the one below.

Kynar Flex® 2800-00

Alternative and trade names
PVDF
Want to keep this datasheet? Save it now in your required format

Description

Kynar Flex® resins are fluorinated thermoplastic copolymers.

Outstanding characteristics: chemical resistance, imperviousness to UV, high barrier properties, high purity, good mechanical and thermo-mechanical properties.

Kynar Flex® 2800-00 resin is a standard grade of granules, compared to the homopolymer grades, which exhibits a lower modulus, a better resistance to stress cracking in alkaline and oxidizing media, and a lower melting point. For cable coating, extrusion of tube and plaque, compression molding of bulky parts.

Additional characteristics:

  • Easily processed using conventional equipment
  • Excellent thermal stability
  • Retains properties after aging
  • Pigmentable
  • UL RTI temperature rating 125ºC
  • Radiation crosslinking

  • This material data has been provided by Arkema Technical Polymers.

    All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
    Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

    Ashby charts

    See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

    Properties

    General

    PropertyValueTesting StandardConditionComment

    Coefficient of friction

    0.33 [-]

    Show Supplier Material materials with Coefficient of friction of 0.33 [-]

    ASTM D1894

    vs Steel, Static

    0.33 [-]

    Show Supplier Material materials with Coefficient of friction of 0.33 [-]

    ASTM D1894

    vs Steel, Kinetic

    Density

    1.77 - 1.8 g/cm³

    Show Supplier Material materials with Density of 1.77 - 1.8 g/cm³

    ASTM D792

    1.78 g/cm³

    Show Supplier Material materials with Density of 1.78 g/cm³

    ISO 1183

    dry

    Limiting oxygen index

    42 %

    Show Supplier Material materials with Limiting oxygen index of 42 %

    ASTM D2863

    43 %

    Show Supplier Material materials with Limiting oxygen index of 43 %

    ISO 4589-1/-2

    dry

    Moisture absorption

    0.015 %

    Show Supplier Material materials with Moisture absorption of 0.015 %

    Sim. to ISO 62

    Water absorption

    0.03 %

    Show Supplier Material materials with Water absorption of 0.03 %

    Sim. to ISO 62

    0.03 - 0.05 %

    Show Supplier Material materials with Water absorption of 0.03 - 0.05 %

    ASTM D570

    Mechanical

    PropertyTemperatureValueTesting StandardConditionComment

    Compressive strength

    31 - 41.4 MPa

    Show Supplier Material materials with Compressive strength of 31 - 41.4 MPa

    ASTM D695

    Elastic modulus

    0.552 - 0.896 GPa

    Show Supplier Material materials with Elastic modulus of 0.552 - 0.896 GPa

    ASTM D638

    0.7 GPa

    Show Supplier Material materials with Elastic modulus of 0.7 GPa

    ISO 527-1/-2

    dry

    Elongation

    50 %

    Show Supplier Material materials with Elongation of 50 %

    ISO 527-1/-2

    dry

    min. | nominal

    100 - 300 %

    Show Supplier Material materials with Elongation of 100 - 300 %

    ASTM D638

    Elongation at yield

    10 - 20 %

    Show Supplier Material materials with Elongation at yield of 10 - 20 %

    ASTM D638

    15 %

    Show Supplier Material materials with Elongation at yield of 15 %

    ISO 527-1/-2

    dry

    Flexural modulus

    0.483 - 0.758 GPa

    Show Supplier Material materials with Flexural modulus of 0.483 - 0.758 GPa

    ASTM D790

    Flexural strength

    20.7 - 34.5 MPa

    Show Supplier Material materials with Flexural strength of 20.7 - 34.5 MPa

    ASTM D790

    at 5% strain

    Hardness, Shore D

    60 - 70 [-]

    Show Supplier Material materials with Hardness, Shore D of 60 - 70 [-]

    ASTM D2240

    Impact strength, Charpy notched

    -30 °C

    5 kJ/m²

    Show Supplier Material materials with Impact strength, Charpy notched of 5 kJ/m²

    ISO 179/1eA

    dry

    No Break at 23°C

    Impact strength, Charpy notched, ASTM

    23 °C

    534 - 1070 J/m

    Show Supplier Material materials with Impact strength, Charpy notched, ASTM of 534 - 1070 J/m

    ASTM D256

    Impact strength, Charpy unnotched, ASTM

    No Break at 23°C

    ASTM D256

    Tensile strength

    17.2 - 34.5 MPa

    Show Supplier Material materials with Tensile strength of 17.2 - 34.5 MPa

    ASTM D638

    Yield strength

    20 - 34.5 MPa

    Show Supplier Material materials with Yield strength of 20 - 34.5 MPa

    ASTM D638

    27 MPa

    Show Supplier Material materials with Yield strength of 27 MPa

    ISO 527-1/-2

    dry

    Thermal

    PropertyValueTesting StandardConditionPressureComment

    Coefficient of thermal expansion

    0.000126 - 0.000185 1/K

    Show Supplier Material materials with Coefficient of thermal expansion of 0.000126 - 0.000185 1/K

    ASTM D696

    0.00016 1/K

    Show Supplier Material materials with Coefficient of thermal expansion of 0.00016 1/K

    ISO 11359-1/-2

    dry

    Glass transition temperature

    -41.1 - -39.4 °C

    Show Supplier Material materials with Glass transition temperature of -41.1 - -39.4 °C

    ASTM D7028

    -40 °C

    Show Supplier Material materials with Glass transition temperature of -40 °C

    ISO 11357-1/-2

    dry

    10°C/min

    Heat deflection temperature

    40 - 55 °C

    Show Supplier Material materials with Heat deflection temperature of 40 - 55 °C

    ASTM D648

    2 MPa

    248 °F/hr

    48 °C

    Show Supplier Material materials with Heat deflection temperature of 48 °C

    ISO 75-1/-2

    dry

    2 MPa

    60 - 75 °C

    Show Supplier Material materials with Heat deflection temperature of 60 - 75 °C

    ASTM D648

    0.45 MPa

    248 °F/hr

    68 °C

    Show Supplier Material materials with Heat deflection temperature of 68 °C

    ISO 75-1/-2

    dry

    0.45 MPa

    Melting point

    140 - 145 °C

    Show Supplier Material materials with Melting point of 140 - 145 °C

    ASTM D3418

    143 °C

    Show Supplier Material materials with Melting point of 143 °C

    ISO 11357-1/-3

    dry

    10°C/min

    Relative temperature index, electrical

    130 °C

    Show Supplier Material materials with Relative temperature index, electrical of 130 °C

    UL 746B

    Relative temperature index, mechanical strength

    130 °C

    Show Supplier Material materials with Relative temperature index, mechanical strength of 130 °C

    UL 746B

    Specific heat capacity

    745 - 958 J/(kg·K)

    Show Supplier Material materials with Specific heat capacity of 745 - 958 J/(kg·K)

    DSC

    Thermal conductivity

    0.144 - 0.18 W/(m·K)

    Show Supplier Material materials with Thermal conductivity of 0.144 - 0.18 W/(m·K)

    ASTM D433

    Thermal decomposition in air

    375 °C

    Show Supplier Material materials with Thermal decomposition in air of 375 °C

    TGA

    1% wt. loss

    Thermal decomposition in nitrogen

    410 °C

    Show Supplier Material materials with Thermal decomposition in nitrogen of 410 °C

    TGA

    1% wt. loss

    Vicat softening temperature

    79 °C

    Show Supplier Material materials with Vicat softening temperature of 79 °C

    ISO 306

    50°C/h 50N

    Flammability

    At thickness 1.5 mm IEC 60695-11-10: V-0, At thickness 0.8 mm IEC 60695-11-10: V-0 and yellow card available

    Electrical

    PropertyValueFrequencyTesting StandardCondition

    Dielectric constant

    3.5 - 10.6 [-]

    Show Supplier Material materials with Dielectric constant of 3.5 - 10.6 [-]

    1KHz

    ASTM D150

    7 [-]

    Show Supplier Material materials with Dielectric constant of 7 [-]

    1MHz

    IEC 60250

    dry

    11 [-]

    Show Supplier Material materials with Dielectric constant of 11 [-]

    100Hz

    IEC 60250

    dry

    Dielectric strength

    51.2 - 59.1 kV/mm

    Show Supplier Material materials with Dielectric strength of 51.2 - 59.1 kV/mm

    ASTM D149

    Dissipation factor

    0.02 - 0.21 [-]

    Show Supplier Material materials with Dissipation factor of 0.02 - 0.21 [-]

    100KHz

    ASTM D150

    0.052 [-]

    Show Supplier Material materials with Dissipation factor of 0.052 [-]

    100Hz

    IEC 60250

    dry

    0.233 [-]

    Show Supplier Material materials with Dissipation factor of 0.233 [-]

    1MHz

    IEC 60250

    dry

    Surface resistivity

    5.1e+11 - 5.3e+11 Ω/sq

    Show Supplier Material materials with Surface resistivity of 5.1e+11 - 5.3e+11 Ω/sq

    ASTM D257

    Volume resistivity

    2e+14 Ω·cm

    Show Supplier Material materials with Volume resistivity of 2e+14 Ω·cm

    ASTM D257

    65% RH

    2e+14 Ω·cm

    Show Supplier Material materials with Volume resistivity of 2e+14 Ω·cm

    IEC 60093

    dry

    Optical

    PropertyValueTesting StandardComment

    Refractive index

    1 [-]

    Show Supplier Material materials with Refractive index of 1 [-]

    ASTM D542

    sodium D line

    Rheological Properties

    PropertyValueTesting StandardConditionComment

    Melt mass-flow rate

    3 - 8 g/10min

    Show Supplier Material materials with Melt mass-flow rate of 3 - 8 g/10min

    ASTM D1238

    230°C/12.5kg

    Melt viscosity

    2700 - 220000 Pa·s

    Show Supplier Material materials with Melt viscosity of 2700 - 220000 Pa·s

    ASTM D3835

    Melt volume-flow rate

    0.5 cm³/10min

    Show Supplier Material materials with Melt volume-flow rate of 0.5 cm³/10min

    ISO 1133

    dry

    230°C/5kg

    Technological properties

    Property
    Application areas

    Fuel Management - Fuel Lines,Fuel Management - In-Tank and Fuel Venting Lines,Chemical Process Industry,Chemical Process Industry - Injection Molding,Chemical Process Industry - Stock Shapes,Tubing and Hoses,Automotive Cables,Performance Wire,PVDF Cable Jacketing,Wire and Cables,Offshore Umbilicals,Underground Fuel Containment

    Processing methods

    Compression Molding:

  • Molding temperature (°C) ISO 293: 225
  • Molding time (min) ISO 293: 3
  • DeMolding temperature (°C) ISO 293: 120