Dimension
Property | Value |
---|---|
Thickness | 20 - 600 mm Show Supplier Material materials with Thickness of 20 - 600 mm |
Width | 350 - 1010 mm Show Supplier Material materials with Width of 350 - 1010 mm |
Mechanical
Property | Value | Comment |
---|---|---|
Hardness, Brinell | 355 - 410 [-] Show Supplier Material materials with Hardness, Brinell of 355 - 410 [-] | as-delivered condition |
Hardness, Rockwell C | 56 - 58 [-] Show Supplier Material materials with Hardness, Rockwell C of 56 - 58 [-] | after quenching |
Tensile strength | 1190 - 1385 MPa Show Supplier Material materials with Tensile strength of 1190 - 1385 MPa |
Thermal
Property | Temperature | Value | Comment |
---|---|---|---|
Coefficient of thermal expansion | 100 °C | 1.22e-05 1/K Show Supplier Material materials with Coefficient of thermal expansion of 1.22e-05 1/K | for 20°C to the mentioned temperature |
200 °C | 1.3e-05 1/K Show Supplier Material materials with Coefficient of thermal expansion of 1.3e-05 1/K | for 20°C to the mentioned temperature | |
300 °C | 1.33e-05 1/K Show Supplier Material materials with Coefficient of thermal expansion of 1.33e-05 1/K | for 20°C to the mentioned temperature | |
400 °C | 1.37e-05 1/K Show Supplier Material materials with Coefficient of thermal expansion of 1.37e-05 1/K | for 20°C to the mentioned temperature | |
500 °C | 1.42e-05 1/K Show Supplier Material materials with Coefficient of thermal expansion of 1.42e-05 1/K | for 20°C to the mentioned temperature | |
600 °C | 1.44e-05 1/K Show Supplier Material materials with Coefficient of thermal expansion of 1.44e-05 1/K | for 20°C to the mentioned temperature | |
Thermal conductivity | 23 °C | 36 W/(m·K) Show Supplier Material materials with Thermal conductivity of 36 W/(m·K) | |
350 °C | 38.8 W/(m·K) Show Supplier Material materials with Thermal conductivity of 38.8 W/(m·K) | ||
700 °C | 35 W/(m·K) Show Supplier Material materials with Thermal conductivity of 35 W/(m·K) |
Chemical properties
Property | Value |
---|---|
Carbon | 0.56 % Show Supplier Material materials with Carbon of 0.56 % |
Chromium | 1.1 % Show Supplier Material materials with Chromium of 1.1 % |
Iron | Balance |
Manganese | 0.75 % Show Supplier Material materials with Manganese of 0.75 % |
Nickel | 1.7 % Show Supplier Material materials with Nickel of 1.7 % |
Silicon | 0.25 % Show Supplier Material materials with Silicon of 0.25 % |
Vanadium | 0.1 % Show Supplier Material materials with Vanadium of 0.1 % |
Technological properties
Property | ||
---|---|---|
Application areas | Standard steel for forging dies, press dies, auxiliary tools for extrusion, die holders, armoured trim dies, hot shear blades | |
Heat Treatment | Soft annealing: 650-700°C (Cooling in furnace) - Hardening: 830-870°C, 860-900 (Oil, Air) |