Formadur PH 42 Superclean Plate

Alternative and trade names
15NiCuAl12-10-10
Want to keep this datasheet? Save it now in your required format

Description

Formadur PH 42 (15NiCuAl12-10-10) Precipitation hardened, remelted plastic mould steel that shows the following features and properties:


  • Exellent polishability
  • Good electrical discharge machinability
  • Good weldability
  • Improved compressive strength due to higher hardness compared to conventional plastic mould steels
  • Suitability for texturing
  • This material data has been provided by Deutsche Edelstahlwerke Specialty Steel (DEW).

    "Typical" values were obtained via a literature search. "Predicted" values were imputed via artificial intelligence technology. While we have placed significant efforts in ensuring data accuracy, "typical" and "predicted" data should be considered indicative and verified by appropriate material testing. Please do contact us if additional information on the the predicted data method is required.
    All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
    Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

    Ashby charts

    Properties

    Dimension

    PropertyValue

    Thickness

    205 mm

    Show Supplier Material materials with Thickness of 205 mm

    Width

    510 mm

    Show Supplier Material materials with Width of 510 mm

    Mechanical

    PropertyValue

    Elastic modulus

    206 GPa

    Show Supplier Material materials with Elastic modulus of 206 GPa

    Hardness, Rockwell C

    36 - 40 [-]

    Show Supplier Material materials with Hardness, Rockwell C of 36 - 40 [-]

    Tensile strength

    1125 - 1255 MPa

    Show Supplier Material materials with Tensile strength of 1125 - 1255 MPa

    Thermal

    PropertyTemperatureValueComment

    Coefficient of thermal expansion

    100 °C

    1.26e-05 1/K

    Show Supplier Material materials with Coefficient of thermal expansion of 1.26e-05 1/K

    for 20°C to the mentioned temperature

    150 °C

    1.28e-05 1/K

    Show Supplier Material materials with Coefficient of thermal expansion of 1.28e-05 1/K

    for 20°C to the mentioned temperature

    200 °C

    1.3e-05 1/K

    Show Supplier Material materials with Coefficient of thermal expansion of 1.3e-05 1/K

    for 20°C to the mentioned temperature

    250 °C

    1.33e-05 1/K

    Show Supplier Material materials with Coefficient of thermal expansion of 1.33e-05 1/K

    for 20°C to the mentioned temperature

    300 °C

    1.35e-05 1/K

    Show Supplier Material materials with Coefficient of thermal expansion of 1.35e-05 1/K

    for 20°C to the mentioned temperature

    350 °C

    1.37e-05 1/K

    Show Supplier Material materials with Coefficient of thermal expansion of 1.37e-05 1/K

    for 20°C to the mentioned temperature

    400 °C

    1.39e-05 1/K

    Show Supplier Material materials with Coefficient of thermal expansion of 1.39e-05 1/K

    for 20°C to the mentioned temperature

    450 °C

    1.4e-05 1/K

    Show Supplier Material materials with Coefficient of thermal expansion of 1.4e-05 1/K

    for 20°C to the mentioned temperature

    500 °C

    1.42e-05 1/K

    Show Supplier Material materials with Coefficient of thermal expansion of 1.42e-05 1/K

    for 20°C to the mentioned temperature

    Thermal conductivity

    23 °C

    25.7 W/(m·K)

    Show Supplier Material materials with Thermal conductivity of 25.7 W/(m·K)

    150 °C

    29.4 W/(m·K)

    Show Supplier Material materials with Thermal conductivity of 29.4 W/(m·K)

    300 °C

    29.8 W/(m·K)

    Show Supplier Material materials with Thermal conductivity of 29.8 W/(m·K)

    350 °C

    29.6 W/(m·K)

    Show Supplier Material materials with Thermal conductivity of 29.6 W/(m·K)

    400 °C

    29.2 W/(m·K)

    Show Supplier Material materials with Thermal conductivity of 29.2 W/(m·K)

    500 °C

    28.2 W/(m·K)

    Show Supplier Material materials with Thermal conductivity of 28.2 W/(m·K)

    Chemical properties

    PropertyValue

    Aluminium

    1 %

    Show Supplier Material materials with Aluminium of 1 %

    Carbon

    0.15 %

    Show Supplier Material materials with Carbon of 0.15 %

    Iron

    Balance

    Manganese

    1.5 %

    Show Supplier Material materials with Manganese of 1.5 %

    Nickel

    3 %

    Show Supplier Material materials with Nickel of 3 %

    Silicon

    0.3 %

    Show Supplier Material materials with Silicon of 0.3 %

    Technological properties

    Property
    Application areas

    Suitable for all kinds of tools in plastic processing with high demands on strength, such as highly stressed plastic injection moulds, compression moulds, hot-runner.

    Heat Treatment

    Formadur PH 42 Superclean is supplied in precipitation hardened condition with a hardness of approx. 38 HRC. No additional heat treatment is necessary. After repair welding an ageing at 520 °C/1 hr is recommended.