General
Property | Value |
---|---|
Bulk density | 4.63 g/cm³ Show Supplier Material materials with Bulk density of 4.63 g/cm³ |
Density | 7.9 g/cm³ Show Supplier Material materials with Density of 7.9 g/cm³ |
Particle size range | 10 - 45 µm Show Supplier Material materials with Particle size range of 10 - 45 µm |
Mechanical
Property | Value | Comment |
---|---|---|
Charpy impact energy, V-notch | 22 J Show Supplier Material materials with Charpy impact energy, V-notch of 22 J | |
Elongation | 27 % Show Supplier Material materials with Elongation of 27 % | A5 |
Hardness, Rockwell C | 27 [-] Show Supplier Material materials with Hardness, Rockwell C of 27 [-] | |
Tensile strength | 1080 MPa Show Supplier Material materials with Tensile strength of 1080 MPa | |
Yield strength | 630 MPa Show Supplier Material materials with Yield strength of 630 MPa | RP02 |
Thermal
Property | Value |
---|---|
Coefficient of thermal expansion | 1.05e-05 1/K Show Supplier Material materials with Coefficient of thermal expansion of 1.05e-05 1/K |
Rheological Properties
Property | Value |
---|---|
Hall flow | 16 s/50g Show Supplier Material materials with Hall flow of 16 s/50g |
Chemical properties
Property | Value |
---|---|
Carbon | 0.14 % Show Supplier Material materials with Carbon of 0.14 % |
Chromium | 28 % Show Supplier Material materials with Chromium of 28 % |
Cobalt | Balance |
Iron | 0.75 % Show Supplier Material materials with Iron of 0.75 % |
Manganese | 1 % Show Supplier Material materials with Manganese of 1 % |
Molybdenum | 6 % Show Supplier Material materials with Molybdenum of 6 % |
Nickel | 0.1 % Show Supplier Material materials with Nickel of 0.1 % |
Nitrogen | 0.25 % Show Supplier Material materials with Nitrogen of 0.25 % |
Silicon | 1 % Show Supplier Material materials with Silicon of 1 % |
Technological properties
Property | ||
---|---|---|
Application areas | Suitable for the production of CoCrMo implants | |
Processing history | The powder is produced by gas atomization. | |
Processing methods | Printdur® CoCrF75 can be processed on LPBF systems. |