Corrodur 4021 QT700

Alternative and trade names
Corrodur 4021, X20Cr13, 1.4021, 420, SUS 420J1, 20X133
Want to keep this datasheet? Save it now in your required format

Description

1.4021 (X20Cr13) is used in the quenched and tempered condition in a host of constructional and fastener applications where moderate corrosion resistance is required. The knife blade variant of 1.4021 can be polished to high gloss finishes. Optimal corrosion resistance is also attained when the surface is finely ground or polished.

Related Standards

Equivalent Materials

This material data has been provided by Deutsche Edelstahlwerke Specialty Steel (DEW).

"Typical" values were obtained via a literature search. "Predicted" values were imputed via artificial intelligence technology. While we have placed significant efforts in ensuring data accuracy, "typical" and "predicted" data should be considered indicative and verified by appropriate material testing. Please do contact us if additional information on the the predicted data method is required.
All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyValue

Density

7.7 g/cm³

Show Supplier Material materials with Density of 7.7 g/cm³

Dimension

PropertyValueComment

Diameter

160 mm

Show Supplier Material materials with Diameter of 160 mm

max.

Mechanical

PropertyTemperatureValueComment

Charpy impact energy, V-notch

25 J

Show Supplier Material materials with Charpy impact energy, V-notch of 25 J

Elastic modulus

20 °C

215 GPa

Show Supplier Material materials with Elastic modulus of 215 GPa

100 °C

212 GPa

Show Supplier Material materials with Elastic modulus of 212 GPa

200 °C

205 GPa

Show Supplier Material materials with Elastic modulus of 205 GPa

300 °C

200 GPa

Show Supplier Material materials with Elastic modulus of 200 GPa

400 °C

190 GPa

Show Supplier Material materials with Elastic modulus of 190 GPa

Elongation

13 %

Show Supplier Material materials with Elongation of 13 %

A5

Hardness, Brinell

230 [-]

Show Supplier Material materials with Hardness, Brinell of 230 [-]

annealed

Tensile strength

700 - 850 MPa

Show Supplier Material materials with Tensile strength of 700 - 850 MPa

Yield strength

20 °C

500 MPa

Show Supplier Material materials with Yield strength of 500 MPa

RP02

100 °C

460 MPa

Show Supplier Material materials with Yield strength of 460 MPa

RP02

150 °C

445 MPa

Show Supplier Material materials with Yield strength of 445 MPa

RP02

200 °C

430 MPa

Show Supplier Material materials with Yield strength of 430 MPa

RP02

250 °C

415 MPa

Show Supplier Material materials with Yield strength of 415 MPa

RP02

300 °C

395 MPa

Show Supplier Material materials with Yield strength of 395 MPa

RP02

350 °C

365 MPa

Show Supplier Material materials with Yield strength of 365 MPa

RP02

400 °C

330 MPa

Show Supplier Material materials with Yield strength of 330 MPa

RP02

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

100 °C

1.05e-05 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 1.05e-05 1/K

for 20°C to the mentioned temperature

200 °C

1.1e-05 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 1.1e-05 1/K

for 20°C to the mentioned temperature

300 °C

1.15e-05 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 1.15e-05 1/K

for 20°C to the mentioned temperature

400 °C

1.2e-05 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 1.2e-05 1/K

for 20°C to the mentioned temperature

Specific heat capacity

460 J/(kg·K)

Show Supplier Material materials with Specific heat capacity of 460 J/(kg·K)

Thermal conductivity

30 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 30 W/(m·K)

Electrical

PropertyValue

Electrical resistivity

6e-07 Ω·m

Show Supplier Material materials with Electrical resistivity of 6e-07 Ω·m

Chemical properties

PropertyValue

Carbon

0.16 - 0.25 %

Show Supplier Material materials with Carbon of 0.16 - 0.25 %

Chromium

12 - 14 %

Show Supplier Material materials with Chromium of 12 - 14 %

Iron

Balance

Manganese

1 %

Show Supplier Material materials with Manganese of 1 %

Molybdenum

0.5 %

Show Supplier Material materials with Molybdenum of 0.5 %

Nickel

0.5 %

Show Supplier Material materials with Nickel of 0.5 %

Phosphorus

0.04 %

Show Supplier Material materials with Phosphorus of 0.04 %

Silicon

1 %

Show Supplier Material materials with Silicon of 1 %

Sulfur

0.01 - 0.03 %

Show Supplier Material materials with Sulfur of 0.01 - 0.03 %

Technological properties

Property
Application areas

Automotive industry, Decorative Applications, Hydraulic Equipment, Petrochemical industry, Food and Beverage industry, Mechanical engineering, Cutlery, Blades

Corrosion properties

Average - Good corrosion resistance in moderately corrosive environments that are free of chlorides, such as soaps, detergents and organic acids. Good resistance in oxidising atmospheres up to temperatures of about 600 °C. 1.4021 is not resistant to intergranular corrosion in the asdelivered or as-welded conditions. PRE = 12.0 – 14.0

General machinability

Good - The machinability of this grade of stainless steel is directly related to its hardness. 1.4021 machines similar to carbon steels of the same hardness. Although it must be realised that the machining parameters will vary depending on the structure/hardness of the steel.

Heat Treatment

Soft annealing: 745-825°C (Cooling in furnace, air) - Hardening: 950-1050°C and quenching in air, polymer, oil - Tempering: 650-750°C

Hot forming

It is formable at 800-1100°C

Processing history

Quenched and tempered, QT 700

Welding

Good - Preheating of the work piece to a temperature within the range 100 °C – 300 °C is required as well as a post weld tempering treatment when welding is performed using a matching filler material. Generally, Novonit® 4551 is recommended when a filler material is required. Tempering at 650 °C after welding is recommended to restore some of the ductility in the weld zone. When using an inert or protective shielding gas during welding, care must be taken to avoid use of any hydrogen or nitrogen containing gases since contamination of the weld with nitrogen or hydrogen will adversely affect the mechanical properties. After welding the work piece must be cooled to below the martensite start (MS), temperature of approximately 120 °C before being tempered.