Acidur 4542 P930

Alternative and trade names
Acidur 4542, 1.4542, Type 630, SUS 630
Want to keep this datasheet? Save it now in your required format

Description

Acidur 4542 (1.4542) is a hardenable stainless steel with high yield strength, high wear resistance and good corrosion resistance. As a remelted variant (ESU/VU) this steel is used in the aerospace industry. It is suitable for low temperatures and can be used up to approx. 315°C

Related Standards

Equivalent Materials

This material data has been provided by Deutsche Edelstahlwerke Specialty Steel (DEW).

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyValue

Density

7.8 g/cm³

Show Supplier Material materials with Density of 7.8 g/cm³

Dimension

PropertyValueComment

Diameter

100 mm

Show Supplier Material materials with Diameter of 100 mm

max.

Mechanical

PropertyTemperatureValueComment

Charpy impact energy, V-notch

40.0 J

Show Supplier Material materials with Charpy impact energy, V-notch of 40.0 J

Elastic modulus

20 °C

200 GPa

Show Supplier Material materials with Elastic modulus of 200 GPa

100 °C

195 GPa

Show Supplier Material materials with Elastic modulus of 195 GPa

200 °C

185 GPa

Show Supplier Material materials with Elastic modulus of 185 GPa

300 °C

175 GPa

Show Supplier Material materials with Elastic modulus of 175 GPa

400 °C

170 GPa

Show Supplier Material materials with Elastic modulus of 170 GPa

Hardness, Brinell

360.0

Show Supplier Material materials with Hardness, Brinell of 360.0

annealed

Tensile strength

930.0 - 1100.0 MPa

Show Supplier Material materials with Tensile strength of 930.0 - 1100.0 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

100 °C

0.0000109 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000109 1/K

for 20°C to the mentioned temperature

200 °C

0.0000111 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000111 1/K

for 20°C to the mentioned temperature

Specific heat capacity

500.0 J/(kg·K)

Show Supplier Material materials with Specific heat capacity of 500.0 J/(kg·K)

Thermal conductivity

16 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 16 W/(m·K)

Electrical

PropertyValue

Electrical resistivity

7.1e-07 Ω·m

Show Supplier Material materials with Electrical resistivity of 7.1e-07 Ω·m

Chemical properties

PropertyValueComment

Carbon

0.07

Show Supplier Material materials with Carbon of 0.07

Chromium

15.0 - 17.0 %

Show Supplier Material materials with Chromium of 15.0 - 17.0 %

Copper

3.0 - 5.0 %

Show Supplier Material materials with Copper of 3.0 - 5.0 %

Manganese

1.0

Show Supplier Material materials with Manganese of 1.0

Molybdenum

0.6000000000000001

Show Supplier Material materials with Molybdenum of 0.6000000000000001

Nickel

3.0 - 5.0 %

Show Supplier Material materials with Nickel of 3.0 - 5.0 %

Other

0.15

Show Supplier Material materials with Other of 0.15

0.45

Phosphorus

0.04

Show Supplier Material materials with Phosphorus of 0.04

Silicon

0.7000000000000001

Show Supplier Material materials with Silicon of 0.7000000000000001

Sulfur

0.03

Show Supplier Material materials with Sulfur of 0.03

Technological properties

Property
Application areas

Aerospace, Plant engineering and construction, Chemical industry, Wood industry, Mechanical engineering, Oil industry, Paper industry, Sports and leisure industry, Ship building

Corrosion properties

The good combination of high corrosion resistance and good mechanical properties makes Acidur 4542 suitable for use in marine environments. In standing seawater, however, Acidur 4542 is susceptible to crevice corrosion. If application in standing seawater cannot be excluded, additional protection (e.g. painting) must be applied.

General machinability

Acidur 4542 can be machined in both the solution annealed and hardened condition. The machinability of Acidur 4542 depends on the hardness

Heat Treatment

Hardening:1030-1055°C in oil, air - Percipitation hardening: 4 hr 620°C in air

Hot forming

It is formable at 900-1150°C

Processing history

Percipitation hardened P930

Welding

To weld Acidur 4542, the condition of the base material must be taken into account. The copper is present in the material in a stable form and therefore does not promote hot cracking. In addition to setting optimum welding conditions, care must be taken to avoid undercuts or other welding defects that lead to the formation of a notch. After welding, the material must be solution annealed again within a very short time with subsequent ageing to prevent stress cracking.