Description

1.4301 is the standard for the austenitic grades of stainless steel due to its good corrosion resistance, ease of formability and fabrication coupled with its aesthetic appearance in the polished, ground and brushed conditions. Since 1.4301 is not resistant to intergranular corrosion in the welded condition, 1.4307 should rather be specified if welding of larger sections is required and no solution annealing treatment after welding can be performed. Surface condition plays an important role in the corrosion resistance of this steel with polished surfaces exhibiting far superior corrosion resistance compared with rougher surfaces on the same material.

Related Standards

Equivalent Materials

This material data has been provided by Deutsche Edelstahlwerke Specialty Steel (DEW).

"Typical" values were obtained via a literature search. "Predicted" values were imputed via artificial intelligence technology. While we have placed significant efforts in ensuring data accuracy, "typical" and "predicted" data should be considered indicative and verified by appropriate material testing. Please do contact us if additional information on the the predicted data method is required.
All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyValue

Density

7.9 g/cm³

Show Supplier Material materials with Density of 7.9 g/cm³

Dimension

PropertyValueComment

Diameter

250 mm

Show Supplier Material materials with Diameter of 250 mm

max.

Mechanical

PropertyTemperatureValueComment

Charpy impact energy, V-notch

100 J

Show Supplier Material materials with Charpy impact energy, V-notch of 100 J

Elastic modulus

20 °C

200 GPa

Show Supplier Material materials with Elastic modulus of 200 GPa

100 °C

194 GPa

Show Supplier Material materials with Elastic modulus of 194 GPa

200 °C

186 GPa

Show Supplier Material materials with Elastic modulus of 186 GPa

300 °C

179 GPa

Show Supplier Material materials with Elastic modulus of 179 GPa

400 °C

172 GPa

Show Supplier Material materials with Elastic modulus of 172 GPa

500 °C

165 GPa

Show Supplier Material materials with Elastic modulus of 165 GPa

Elongation

35 %

Show Supplier Material materials with Elongation of 35 %

A5 | Transverse

45 %

Show Supplier Material materials with Elongation of 45 %

A5

Hardness, Brinell

215 [-]

Show Supplier Material materials with Hardness, Brinell of 215 [-]

Tensile strength

500 - 700 MPa

Show Supplier Material materials with Tensile strength of 500 - 700 MPa

Yield strength

20 °C

190 MPa

Show Supplier Material materials with Yield strength of 190 MPa

RP02

23 °C

225 MPa

Show Supplier Material materials with Yield strength of 225 MPa

RP1

100 °C

155 MPa

Show Supplier Material materials with Yield strength of 155 MPa

RP02

100 °C

190 MPa

Show Supplier Material materials with Yield strength of 190 MPa

RP1

150 °C

140 MPa

Show Supplier Material materials with Yield strength of 140 MPa

RP02

150 °C

170 MPa

Show Supplier Material materials with Yield strength of 170 MPa

RP1

200 °C

127 MPa

Show Supplier Material materials with Yield strength of 127 MPa

RP02

200 °C

155 MPa

Show Supplier Material materials with Yield strength of 155 MPa

RP1

250 °C

118 MPa

Show Supplier Material materials with Yield strength of 118 MPa

RP02

250 °C

145 MPa

Show Supplier Material materials with Yield strength of 145 MPa

RP1

300 °C

110 MPa

Show Supplier Material materials with Yield strength of 110 MPa

RP02

300 °C

135 MPa

Show Supplier Material materials with Yield strength of 135 MPa

RP1

350 °C

104 MPa

Show Supplier Material materials with Yield strength of 104 MPa

RP02

350 °C

129 MPa

Show Supplier Material materials with Yield strength of 129 MPa

RP1

400 °C

98 MPa

Show Supplier Material materials with Yield strength of 98 MPa

RP02

400 °C

125 MPa

Show Supplier Material materials with Yield strength of 125 MPa

RP1

450 °C

95 MPa

Show Supplier Material materials with Yield strength of 95 MPa

RP02

450 °C

122 MPa

Show Supplier Material materials with Yield strength of 122 MPa

RP1

500 °C

95 MPa

Show Supplier Material materials with Yield strength of 95 MPa

RP02

500 °C

120 MPa

Show Supplier Material materials with Yield strength of 120 MPa

RP1

550 °C

90 MPa

Show Supplier Material materials with Yield strength of 90 MPa

RP02

550 °C

120 MPa

Show Supplier Material materials with Yield strength of 120 MPa

RP1

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

100 °C

1.6e-05 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 1.6e-05 1/K

for 20°C to the mentioned temperature

200 °C

1.65e-05 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 1.65e-05 1/K

for 20°C to the mentioned temperature

300 °C

1.7e-05 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 1.7e-05 1/K

for 20°C to the mentioned temperature

400 °C

1.75e-05 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 1.75e-05 1/K

for 20°C to the mentioned temperature

500 °C

1.8e-05 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 1.8e-05 1/K

for 20°C to the mentioned temperature

Specific heat capacity

500 J/(kg·K)

Show Supplier Material materials with Specific heat capacity of 500 J/(kg·K)

Thermal conductivity

15 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 15 W/(m·K)

Electrical

PropertyValue

Electrical resistivity

7.3e-07 Ω·m

Show Supplier Material materials with Electrical resistivity of 7.3e-07 Ω·m

Chemical properties

PropertyValue

Carbon

0.07 %

Show Supplier Material materials with Carbon of 0.07 %

Chromium

17.5 - 19.5 %

Show Supplier Material materials with Chromium of 17.5 - 19.5 %

Iron

Balance

Manganese

2 %

Show Supplier Material materials with Manganese of 2 %

Nickel

8 - 10.5 %

Show Supplier Material materials with Nickel of 8 - 10.5 %

Nitrogen

0.1 %

Show Supplier Material materials with Nitrogen of 0.1 %

Phosphorus

0.045 %

Show Supplier Material materials with Phosphorus of 0.045 %

Silicon

1 %

Show Supplier Material materials with Silicon of 1 %

Sulfur

0.03 %

Show Supplier Material materials with Sulfur of 0.03 %

Technological properties

Property
Application areas

Automotive industry, Building and Construction industry, Chemical industry, Food and Beverage industry, Decorative items and Kitchen Utensils, Electronic Equipment, Petrochemical industry

Corrosion properties

Good - Due to the moderate carbon content of 1.4301, this grade of stainless steel is prone to sensitisation. The formation of chromium carbides and the associated chromium depleted regions that form around these precipitates make this grade of steel susceptible to intergranular corrosion. Although no danger of intergranular corrosion exists in the supplied (solution annealed) condition, intergranular corrosion may occur after welding or high temperature processing. 1.4301 is resistant to corrosion in most environments provided the chloride and salt concentrations are low. 1.4301 is not recommended for applications where it comes into contact with sea water, nor is it recommended for use in swimming pools. PRE = 17.5 – 21.36

General machinability

Average - For applications which require machining, the NIRO-CUT® 4301 grade is recommended since the composition and production route followed to produce this grade compensates for the work hardening tendency of the material.

Heat Treatment

Optimal material properties are realised after solution annealing in the temperature range 1000 °C – 1100 °C followed by rapid cooling in air or water. Since this grade of steel is susceptible to precipitation of chromium carbides, care must be taken to limit the time spent in the temperature range 450 °C to 850 °C, both during fabrication and service.

Hot forming

It is formable at 900-1200°C

Processing history

Solution Annealed

Welding

Excellent - 1.4301 is weldable with or without the use of filler material. If the use of a filler metal is required, then the use of Novonit® 4316 (AISI 308L) would be recommended. Maximum interpass temperature 200 °C. Post weld heat treatment is not necessary.