General
Property | Temperature | Value |
---|---|---|
Density | 23.0 °C | 8.12 g/cm³ Show Material materials with Density of 8.12 g/cm³ |
Dimension
Property | Value |
---|---|
Length | 1828 mm Show Material materials with Length of 1828 mm |
Thickness | 4.8 - 7.1 mm Show Material materials with Thickness of 4.8 - 7.1 mm |
Width | 381 mm Show Material materials with Width of 381 mm |
Dimensions | Available thicknesses: 4.8mm, 7.1mm |
Mechanical
Property | Temperature | Value | Comment |
---|---|---|---|
Elastic modulus | 23.0 °C | 148 GPa Show Material materials with Elastic modulus of 148 GPa | |
Elongation | 23.0 °C | 30 % Show Material materials with Elongation of 30 % | in 2 in. |
Hardness, Rockwell B | 23.0 °C | 80 [-] Show Material materials with Hardness, Rockwell B of 80 [-] | |
Tensile strength | 23.0 °C | 566 MPa Show Material materials with Tensile strength of 566 MPa | |
Yield strength | 23.0 °C | 235 MPa Show Material materials with Yield strength of 235 MPa |
Thermal
Property | Temperature | Value | Comment |
---|---|---|---|
Coefficient of thermal expansion | 100.0 °C | 4.2E-6 1/K Show Material materials with Coefficient of thermal expansion of 4.2E-6 1/K | from 30°C to the mentioned temperature |
150.0 °C | 4.2E-6 1/K Show Material materials with Coefficient of thermal expansion of 4.2E-6 1/K | from 30°C to the mentioned temperature | |
200.0 °C | 4.2E-6 1/K Show Material materials with Coefficient of thermal expansion of 4.2E-6 1/K | from 30°C to the mentioned temperature | |
250.0 °C | 4.2E-6 1/K Show Material materials with Coefficient of thermal expansion of 4.2E-6 1/K | from 30°C to the mentioned temperature | |
300.0 °C | 4E-6 - 4.7E-6 1/K Show Material materials with Coefficient of thermal expansion of 4E-6 - 4.7E-6 1/K | from 30°C to the mentioned temperature | |
325.0 °C | 4.6E-6 1/K Show Material materials with Coefficient of thermal expansion of 4.6E-6 1/K | from 30°C to the mentioned temperature | |
350.0 °C | 5E-6 1/K Show Material materials with Coefficient of thermal expansion of 5E-6 1/K | from 30°C to the mentioned temperature | |
375.0 °C | 5.6E-6 1/K Show Material materials with Coefficient of thermal expansion of 5.6E-6 1/K | from 30°C to the mentioned temperature | |
400.0 °C | 6.1E-6 1/K Show Material materials with Coefficient of thermal expansion of 6.1E-6 1/K | from 30°C to the mentioned temperature | |
425.0 °C | 6.7E-6 1/K Show Material materials with Coefficient of thermal expansion of 6.7E-6 1/K | from 30°C to the mentioned temperature | |
450.0 °C | 6.7E-6 - 7.4E-6 1/K Show Material materials with Coefficient of thermal expansion of 6.7E-6 - 7.4E-6 1/K | from 30°C to the mentioned temperature | |
475.0 °C | 7.7E-6 1/K Show Material materials with Coefficient of thermal expansion of 7.7E-6 1/K | from 30°C to the mentioned temperature | |
500.0 °C | 8.1E-6 1/K Show Material materials with Coefficient of thermal expansion of 8.1E-6 1/K | from 30°C to the mentioned temperature | |
525.0 °C | 8.5E-6 1/K Show Material materials with Coefficient of thermal expansion of 8.5E-6 1/K | from 30°C to the mentioned temperature | |
550.0 °C | 8.9E-6 1/K Show Material materials with Coefficient of thermal expansion of 8.9E-6 1/K | from 30°C to the mentioned temperature | |
600.0 °C | 9.6E-6 1/K Show Material materials with Coefficient of thermal expansion of 9.6E-6 1/K | from 30°C to the mentioned temperature | |
700.0 °C | 1.05E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.05E-5 1/K | from 30°C to the mentioned temperature | |
800.0 °C | 1.14E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.14E-5 1/K | from 30°C to the mentioned temperature | |
900.0 °C | 1.23E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.23E-5 1/K | from 30°C to the mentioned temperature | |
1004.0 °C | 1.32E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.32E-5 1/K | from 30°C to the mentioned temperature | |
Melting point | 1427 °C Show Material materials with Melting point of 1427 °C | ||
Specific heat capacity | 23.0 °C | 502 J/(kg·K) Show Material materials with Specific heat capacity of 502 J/(kg·K) | |
Thermal conductivity | 23.0 °C | 11 W/(m·K) Show Material materials with Thermal conductivity of 11 W/(m·K) |
Electrical
Property | Temperature | Value |
---|---|---|
Electrical resistivity | 23.0 °C | 6.8E-7 Ω·m Show Material materials with Electrical resistivity of 6.8E-7 Ω·m |
Magnetic
Property | Value |
---|---|
Curie temperature | 380 °C Show Material materials with Curie temperature of 380 °C |
Chemical properties
Property | Value |
---|---|
Carbon | 0.05 % Show Material materials with Carbon of 0.05 % |
Chromium | 0.03 % Show Material materials with Chromium of 0.03 % |
Iron | Balance |
Nickel | 41 % Show Material materials with Nickel of 41 % |
Silicon | 0.3 % Show Material materials with Silicon of 0.3 % |
Sulfur | 0.025 % Show Material materials with Sulfur of 0.025 % |
Technological properties
Property | ||
---|---|---|
Application areas | Common applications of Alloy 42: Thermostats, thermoswitches, integrated circuit lead frames, Glass to metal seals for a wide variety of electronic tubes, hermetic packages, and automotive and industrial lamps., high temperature curing of aircraft thermoset composites |