Property | Value | Comment |
---|---|---|
Density | 1.03 g/cm³ Show Supplier Material materials with Density of 1.03 g/cm³ | ISO 1183 |
Water absorption | 1.1 % Show Supplier Material materials with Water absorption of 1.1 % | ISO 62 |
Mechanical
Property | Value | Comment | |
---|---|---|---|
Elongation | 10 % Show Supplier Material materials with Elongation of 10 % | ISO 527 | |
Flexural strength | 90 MPa Show Supplier Material materials with Flexural strength of 90 MPa | DIN 53452 | |
Hardness, Ball Indentation | 106 MPa Show Supplier Material materials with Hardness, Ball Indentation of 106 MPa | DIN 53452 | |
Hardness, Shore D | 78 [-] Show Supplier Material materials with Hardness, Shore D of 78 [-] | DIN 53505 | |
Impact strength, Charpy notched | 8 - 12 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 8 - 12 kJ/m² | ISO 179 | |
Impact strength, Charpy unnotched | 110 kJ/m² Show Supplier Material materials with Impact strength, Charpy unnotched of 110 kJ/m² | ISO 179 | |
Tear strength | No break, ISO 527 |
Thermal
Property | Value | Pressure | Comment | ||
---|---|---|---|---|---|
Coefficient of thermal expansion | 8e-05 - 0.0001 1/K Show Supplier Material materials with Coefficient of thermal expansion of 8e-05 - 0.0001 1/K | DIN 52328 | |||
Heat deflection temperature | 185 °C Show Supplier Material materials with Heat deflection temperature of 185 °C | 0.45 MPa | |||
190 °C Show Supplier Material materials with Heat deflection temperature of 190 °C | 0.45 MPa | ||||
Max service temperature | 120 °C Show Supplier Material materials with Max service temperature of 120 °C | Longterm | |||
Long | |||||
Short | |||||
Min service temperature | -50 °C Show Supplier Material materials with Min service temperature of -50 °C | Longterm | |||
Thermal conductivity | 0.23 W/(m·K) Show Supplier Material materials with Thermal conductivity of 0.23 W/(m·K) | DIN 52612 | |||
Vicat softening temperature | 182 °C Show Supplier Material materials with Vicat softening temperature of 182 °C | ISO 306, VST B50 | |||
190 °C Show Supplier Material materials with Vicat softening temperature of 190 °C | ISO 306, VST B50 | ||||
Flammability | HB UL 94 |
Electrical
Property | Value | Comment |
---|---|---|
Dielectric constant | 3.5 [-] Show Supplier Material materials with Dielectric constant of 3.5 [-] | DIN 53483 |
Dielectric strength | 30 kV/mm Show Supplier Material materials with Dielectric strength of 30 kV/mm | DIN53480 |
Loss tangent | 0.038 [-] Show Supplier Material materials with Loss tangent of 0.038 [-] | DIN 53483 |
Surface resistivity | 1e+13 Ω/sq Show Supplier Material materials with Surface resistivity of 1e+13 Ω/sq | DIN 53482 |
Volume resistivity | 2.7e+14 Ω·cm Show Supplier Material materials with Volume resistivity of 2.7e+14 Ω·cm | DIN 53482 |
Technological properties
Property | ||
---|---|---|
Certifications | RoHS,REACH |