3M™ Dyneon™ (Fluoroplastic PVDF 110080001)

Want to keep this datasheet? Save it now in your required format

Description

Polyvinylidene Fluoride (PVDF) is ideal for multiple applications across a wide array of industries. Widely used in the chemical processing, wire and cable, semiconductor, and oil and gas industries. PVDF is also gaining recognition in automotive, building, electronics, food processing, pharmaceutical and battery applications.

PVDF 110080001 combines excellent chemical resistance, dimensional stability and excellent flame and smoke resistance with a moderate degree of flexibility. (For applications requiring high degrees of flexibility, see our 30000 series copolymers.)


Special Features are:

  • Copolymer of vinylidene fluoride (VF2) and hexafluoropropylene (HFP)
  • Improved flexibility over PVDF homopolymers
  • Ideal for applications where high strength and a moderate degree of flexibility are required
  • Ideal for high speed extrusion
  • Excellent weatherability
  • Good chemical resistance
  • Long term use temperatures up to 150 °C
  • Processable using most conventional thermoplastic conversion techniques

  • Typical Properties:

    PVDF 110080001 has excellent chemical resistance to most aggressive substances and solvents. As with all 3M PVDF products, PVDF 110080001 has outstanding mechanical strength and toughness, high abrasion resistance, as well as exceptional aging resistance, resistance to UV and nuclear radiation, and low permeability to most gases and liquids. PVDF 110080001 possesses excellent low flame and low smoke properties and is capable of operating in temperatures up to 150°C.

    This material data has been provided by Matmatch.

    All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
    Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

    Ashby charts

    Properties

    General

    PropertyTemperatureValueComment

    Density

    23.0 °C

    1.78 g/cm³

    Show Material materials with Density of 1.78 g/cm³

    ISO 1183

    Water absorption

    23.0 °C

    0.04 %

    Show Material materials with Water absorption of 0.04 %

    ISO 62 (Method 1, 24hr @ 23°C), maximum

    Mechanical

    PropertyTemperatureValueComment

    Elongation

    23.0 °C

    600 %

    Show Material materials with Elongation of 600 %

    ASTM D638, 23 °C, 50 mm/min

    Flexural modulus

    23.0 °C

    1 GPa

    Show Material materials with Flexural modulus of 1 GPa

    ASTM D790

    Tensile strength

    23.0 °C

    47 MPa

    Show Material materials with Tensile strength of 47 MPa

    ASTM D638, 23 °C, 50 mm/min

    Thermal

    PropertyValueComment

    Melting point

    160 °C

    Show Material materials with Melting point of 160 °C

    ASTM D3418

    Rheological Properties

    PropertyValueComment

    Melt mass-flow rate

    24.8 g/10min

    Show Material materials with Melt mass-flow rate of 24.8 g/10min

    ASTM D1238, 230 °C, 5kg, 2.16 kg

    Technological properties

    Property
    Application areas

    PVDF 110080001 has set the standard for plenum rating jacketing and tubes, consistently achieving UL 150°C rating in numerous cable constructions and fibre raceway designs.

    Processing methods

    Injection Molding