Description

High heat PC/ABS blend offering good flow and excellent impact.

This material data has been provided by Matmatch.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

Properties

Mechanical

PropertyTemperatureValueComment

Elastic modulus

23.0 °C

2.25 GPa

Show Material materials with Elastic modulus of 2.25 GPa

ASTM D 638 | 50 mm/min

Elongation

23.0 °C

93 %

Show Material materials with Elongation of 93 %

ASTM D 638 | Type I, 50 mm/min

Elongation at yield

23.0 °C

4.8 %

Show Material materials with Elongation at yield of 4.8 %

ASTM D 638 | Type I, 50 mm/min

Flexural modulus

23.0 °C

2.14 GPa

Show Material materials with Flexural modulus of 2.14 GPa

ISO 178 | 2 mm/min

Flexural yield strength

23.0 °C

81 MPa

Show Material materials with Flexural yield strength of 81 MPa

ISO 178 | 2 mm/min

Impact strength, Charpy notched

23.0 °C

56 kJ/m²

Show Material materials with Impact strength, Charpy notched of 56 kJ/m²

ISO 179/1eA

Impact strength, Izod notched

-30.0 °C

37 kJ/m²

Show Material materials with Impact strength, Izod notched of 37 kJ/m²

ISO 180/1A

23.0 °C

40 - 45 kJ/m²

Show Material materials with Impact strength, Izod notched of 40 - 45 kJ/m²

ISO 180/1A

Impact strength, Izod notched, ASTM

-30.0 °C

425 J/m

Show Material materials with Impact strength, Izod notched, ASTM of 425 J/m

ASTM D 256

23.0 °C

583 J/m

Show Material materials with Impact strength, Izod notched, ASTM of 583 J/m

ASTM D 256

Unlock all property charts

Tensile strength

23.0 °C

45 MPa

Show Material materials with Tensile strength of 45 MPa

ASTM D 638 | Type I, 50 mm/min

Yield strength

23.0 °C

53 MPa

Show Material materials with Yield strength of 53 MPa

ASTM D 638 | Type I, 50 mm/min

Thermal

PropertyValueComment

Heat deflection temperature, 0.45 MPa

128 °C

Show Material materials with Heat deflection temperature, 0.45 MPa of 128 °C

ISO 75/Bf | 0.45 MPa

Vicat softening temperature

121 °C

Show Material materials with Vicat softening temperature of 121 °C

ISO 306 | Rate B/50

Rheological Properties

PropertyValueComment

Melt mass-flow rate

17 g/10min

Show Material materials with Melt mass-flow rate of 17 g/10min

ASTM D 1238 | 260°C/5.0 kgf

Melt volume-flow rate

18 cm³/10min

Show Material materials with Melt volume-flow rate of 18 cm³/10min

ISO 1133 | 260°C/5.0 kg

Technological properties

Property
Application areas

Pharmaceutical Packaging & Drug Delivery

Processing methods

Drying Temperature: 100-110°C, Drying Time: 2-4hrs, Maximum Moisture Content: 0.02%, Melt Temperature: 260-290°C, Nozzle Temperature: 240-280°C, Front - Zone 3 Temperature: 250-290°C, Middle - Zone 2 Temperature: 250-290°C, Rear - Zone 1 Temperature: 230-260°C, Hopper Temperature: 60-80°C, Mold Temperature: 60-90°C