Crastin® HR5315HFS BK591

Alternative and trade names
PBT-I-GF15
Want to keep this datasheet? Save it now in your required format

Description

Common features of Crastin® thermoplastic polyester resin include mechanical and physical properties such as stiffness and toughness, heat resistance, friction and wear resistance, excellent surface finishes and good colourability. Crastin® thermoplastic polyester resin has excellent electrical insulation characteristics and high arc-resistant grades are available. Many flame retardant grades have UL recognition (class V-0). Crastin® thermoplastic polyester resin typically has high chemical and heat ageing resistance. The good melt stability of Crastin® thermoplastic polyester resin normally enables the recycling of properly handled production waste.If recycling is not possible, DuPont recommends, as the preferred option, incineration with energy recovery (-24 kJ/g of base polymer) in appropriately equipped installations. For disposal, local regulations have to be observed. Crastin® thermoplastic polyester resin typically is used in demanding applications in the electronics, electrical, automotive, mechanical engineering, chemical, domestic appliances and sporting goods industry.Crastin® HR5315HFS is a 15% glass reinforced PBT with high flow, moderately toughened, hydrolysis resistant (HR) polybutylene terephtalate for injection molding.

This material data has been provided by Matmatch.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueComment

Density

23.0 °C

1.38 g/cm³

Show Material materials with Density of 1.38 g/cm³

ISO 1183

Water absorption

23.0 °C

0.4 %

Show Material materials with Water absorption of 0.4 %

Sim. to ISO 62 | 80mil

Mechanical

PropertyTemperatureValueComment

Elastic modulus

23.0 °C

5 GPa

Show Material materials with Elastic modulus of 5 GPa

ISO 527-1/-2

Elongation

23.0 °C

3.3 %

Show Material materials with Elongation of 3.3 %

ISO 527-1/-2

Flexural strength

23.0 °C

143 MPa

Show Material materials with Flexural strength of 143 MPa

ISO 178

Impact strength, Charpy notched

-6.0 °C

6 kJ/m²

Show Material materials with Impact strength, Charpy notched of 6 kJ/m²

ISO 179/1eA

23.0 °C

11 kJ/m²

Show Material materials with Impact strength, Charpy notched of 11 kJ/m²

ISO 179/1eA

Impact strength, Charpy unnotched

23.0 °C

57 kJ/m²

Show Material materials with Impact strength, Charpy unnotched of 57 kJ/m²

ISO 179/1eU

Poisson's ratio

23.0 °C

0.35 [-]

Show Material materials with Poisson's ratio of 0.35 [-]

Tensile strength

23.0 °C

95 MPa

Show Material materials with Tensile strength of 95 MPa

ISO 527-1/-2

Thermal

PropertyValueComment

Glass transition temperature

65 °C

Show Material materials with Glass transition temperature of 65 °C

ISO 11357-1/-2 | 18°F/min

Heat deflection temperature, 0.45 MPa

220 °C

Show Material materials with Heat deflection temperature, 0.45 MPa of 220 °C

ISO 75-1/-2

Heat deflection temperature, 1.80 MPa

200 °C

Show Material materials with Heat deflection temperature, 1.80 MPa of 200 °C

ISO 75-1/-2

Melting point

225 °C

Show Material materials with Melting point of 225 °C

ISO 11357-1/-3 | 18°F/min

Relative temperature index, mechanical strength

186 °C

Show Material materials with Relative temperature index, mechanical strength of 186 °C

IEC 60216-1 | 5000 hours

Flammability

Burning Behav. at 60mil nom. thickn.: HB class, Thickness tested: 1.5 mm, Oxygen index: 20 %, FMVSS Class: B -, Burning rate, Thickness 1 mm: 32 mm/min

Electrical

PropertyTemperatureValueComment

Comparative tracking index

23.0 °C

575 V

Show Material materials with Comparative tracking index of 575 V

IEC 60112

Dielectric strength

23.0 °C

35 kV/mm

Show Material materials with Dielectric strength of 35 kV/mm

IEC 60243-1

Dissipation factor, 100Hz

23.0 °C

0.01 [-]

Show Material materials with Dissipation factor, 100Hz of 0.01 [-]

IEC 62631-2-1

Dissipation factor, 1MHz

23.0 °C

0.01 [-]

Show Material materials with Dissipation factor, 1MHz of 0.01 [-]

IEC 62631-2-1

Surface resistivity

23.0 °C

3.00E+13 Ω/sq

Show Material materials with Surface resistivity of 3.00E+13 Ω/sq

IEC 62631-3-2

Volume resistivity

23.0 °C

1.00E+15 Ω·cm

Show Material materials with Volume resistivity of 1.00E+15 Ω·cm

min. | IEC 62631-3-1

Rheological Properties

PropertyTemperatureValueComment

Melt mass-flow rate

18 g/10min

Show Material materials with Melt mass-flow rate of 18 g/10min

ISO 1133 | 250°C/2.16kg

Melt viscosity

250.0 °C

175 Pa·s

Show Material materials with Melt viscosity of 175 Pa·s

ISO 11443 | @ 1000 sec-1, 250°C

Melt volume-flow rate

13 cm³/10min

Show Material materials with Melt volume-flow rate of 13 cm³/10min

ISO 1133

Shrinkage

23.0 °C

0.5 %

Show Material materials with Shrinkage of 0.5 %

ISO 294-4, 2577

Shrinkage, transverse

23.0 °C

1.1 %

Show Material materials with Shrinkage, transverse of 1.1 %

ISO 294-4, 2577

Technological properties

Property
Fillers

15% Glass Fiber

Processing methods

Drying Recommended: yes, Drying Temperature: 120°C, Drying Time, Dehumidified Dryer: 2-4h, Processing Moisture Content: ≤0.04%, Melt Temperature Optimum: 250°C, Min. melt temperature: 240°C, Max. melt temperature: 260°C, Mold Temperature Optimum: 80°C, Min. mold temperature: 30°C, Max. mold temperature: 130°C, Hold pressure range: ≥60MPa, Hold pressure time: 3s/mm, Back pressure: As low as possible, Ejection temperature: 170°C