The material: 'Invar® 36 Sheet' you were looking for has been superseded by the one below.

Invar® 36 Sheet

Alternative and trade names
Invar 36®, Pernifer 36®, Nilo 36®, Invar Steel
Want to keep this datasheet? Save it now in your required format

Description

Invar® is a low expansion alloy consisting of 36% nickel, balance iron.

Related Standards

Equivalent Materials

This material data has been provided by Matmatch.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyValueTemperature

Density

8.05 g/cm³

Show Material materials with Density of 8.05 g/cm³ at 23.0 °C

23.0 °C

Dimension

PropertyValue

Dimensions

Available thicknesses: 0.8mm, 1.0mm, 1.6mm, 2.5mm, 3.2mm

Length

1828 mm

Show Material materials with Length of 1828 mm

Thickness

0.76 - 3.18 mm

Show Material materials with Thickness of 0.76 - 3.18 mm

Width

609.6 mm

Show Material materials with Width of 609.6 mm

Mechanical

PropertyValueTemperatureComment

Elastic modulus

141 GPa

Show Material materials with Elastic modulus of 141 GPa at 23.0 °C

23.0 °C

Elongation

34 %

Show Material materials with Elongation of 34 % at 23.0 °C

23.0 °C

in 2 in.

Hardness, Rockwell B

80 [-]

Show Material materials with Hardness, Rockwell B of 80 [-] at 23.0 °C

23.0 °C

Poisson's ratio

0.29 [-]

Show Material materials with Poisson's ratio of 0.29 [-] at 23.0 °C

23.0 °C

Tensile strength

518 MPa

Show Material materials with Tensile strength of 518 MPa at 23.0 °C

23.0 °C

Yield strength

276 MPa

Show Material materials with Yield strength of 276 MPa at 23.0 °C

23.0 °C

Thermal

PropertyValueTemperatureComment

Coefficient of thermal expansion

1.9E-6 1/K

Show Material materials with Coefficient of thermal expansion of 1.9E-6 1/K at 100.0 °C

100.0 °C

from 20°C to the mentioned temperature

2.4E-6 1/K

Show Material materials with Coefficient of thermal expansion of 2.4E-6 1/K at 150.0 °C

150.0 °C

from 20°C to the mentioned temperature

3E-6 1/K

Show Material materials with Coefficient of thermal expansion of 3E-6 1/K at 200.0 °C

200.0 °C

from 20°C to the mentioned temperature

4.4E-6 1/K

Show Material materials with Coefficient of thermal expansion of 4.4E-6 1/K at 250.0 °C

250.0 °C

from 20°C to the mentioned temperature

6.1E-6 1/K

Show Material materials with Coefficient of thermal expansion of 6.1E-6 1/K at 300.0 °C

300.0 °C

from 20°C to the mentioned temperature

7.5E-6 1/K

Show Material materials with Coefficient of thermal expansion of 7.5E-6 1/K at 350.0 °C

350.0 °C

from 20°C to the mentioned temperature

8.7E-6 1/K

Show Material materials with Coefficient of thermal expansion of 8.7E-6 1/K at 400.0 °C

400.0 °C

from 20°C to the mentioned temperature

8.9E-6 1/K

Show Material materials with Coefficient of thermal expansion of 8.9E-6 1/K at 450.0 °C

450.0 °C

from 20°C to the mentioned temperature

1.05E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.05E-5 1/K at 500.0 °C

500.0 °C

from 20°C to the mentioned temperature

1.18E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.18E-5 1/K at 600.0 °C

600.0 °C

from 20°C to the mentioned temperature

Melting point

1427 °C

Show Material materials with Melting point of 1427 °C

Specific heat capacity

502 J/(kg·K)

Show Material materials with Specific heat capacity of 502 J/(kg·K) at 23.0 °C

23.0 °C

Thermal conductivity

10 W/(m·K)

Show Material materials with Thermal conductivity of 10 W/(m·K) at 23.0 °C

23.0 °C

Electrical

PropertyValueTemperature

Electrical resistivity

8.2E-7 Ω·m

Show Material materials with Electrical resistivity of 8.2E-7 Ω·m at 23.0 °C

23.0 °C

Magnetic

PropertyValue

Curie temperature

279 °C

Show Material materials with Curie temperature of 279 °C

Chemical properties

Property

Carbon

0.05 %

Chromium

0.25 %

Cobalt

0.5 %

Iron

Balance

Nickel

36 %

Silicon

0.4 %

Sulfur

0.015 %

Technological properties

Property
Application areas

Positioning devices • Bimetal thermostats • Advanced composite molds for aerospace industry • Dimensionally stable instruments and optical devices • Containers for LNG tankers • Transfer lines for LNG • Echo boxes and filters for mobile telephones • Magnetic shielding • Small electrical transformers • Metrology devices • Scientific instruments • Electrical circuit breakers • Temperature regulators • Clock balance wheels • Pendulum clocks • Precision condenser blades • Radar and microwave cavity resonators • Special electronic housings • Seals, spacers, and specialized frames • High voltage transmission lines • CRT applications: shadow masks, deflection clips, and electron gun components.