EN 573-3 Grade AW-2014 T6

Want to keep this datasheet? Save it now in your required format

Description

EN AW-2014 is an alloy with strength, machinability and welding capabilities, Aluminum Alloy EN AW-2014 is an excellent option. It is a precipitation hardening alloy that maintains strength after heat treatment.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

2.8 g/cm³

Show Material materials with Density of 2.8 g/cm³

T6

EN 573-3, EN 485, EN 586, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar

20.0 °C

2.8 g/cm³

Show Material materials with Density of 2.8 g/cm³

T6

EN 573-3

Forging, Profile, Rod, Flat, Tube, Sheet

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Bending Fatigue Strength

145.0 MPa

Show Material materials with Bending Fatigue Strength of 145.0 MPa

T6

EN 573-3, EN 485, EN 586, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar

Bending angle 90°

5.0 °/t

Show Material materials with Bending angle 90° of 5.0 °/t

T6

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Bar

7.0 °/t

Show Material materials with Bending angle 90° of 7.0 °/t

T6

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Bar

10.0 °/t

Show Material materials with Bending angle 90° of 10.0 °/t

T6

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Bar

Elastic modulus

-269.0 °C

82.2 GPa

Show Material materials with Elastic modulus of 82.2 GPa

T6

EN 573-3

-195.0 °C

81.8 GPa

Show Material materials with Elastic modulus of 81.8 GPa

T6

EN 573-3

73.0 GPa

Show Material materials with Elastic modulus of 73.0 GPa

T6

EN 573-3, EN 485, EN 586, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar

20.0 °C

72.0 GPa

Show Material materials with Elastic modulus of 72.0 GPa

T6

EN 573-3

Forging, Profile, Rod, Flat, Tube, Sheet

27.0 °C

74.4 GPa

Show Material materials with Elastic modulus of 74.4 GPa

T6

EN 573-3

Elongation

2.0 %

Show Material materials with Elongation of 2.0 %

T6

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Bar

A100

3.0 %

Show Material materials with Elongation of 3.0 %

T6

EN 573-3, EN 586

Strip, Sheet, Plate, Forging, Tube, Bar

A100

4.0 %

Show Material materials with Elongation of 4.0 %

T6

EN 573-3, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar

A50

4.0 %

Show Material materials with Elongation of 4.0 %

T6

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Bar

A100

5.0 %

Show Material materials with Elongation of 5.0 %

T6

EN 573-3, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar

A50

5.0 %

Show Material materials with Elongation of 5.0 %

T6

EN 573-3, EN 485, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar

A100

6.0 %

Show Material materials with Elongation of 6.0 %

T6

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Forging, Tube, Bar

A50

6.0 %

Show Material materials with Elongation of 6.0 %

T6

EN 573-3, EN 485, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar

A100

7.0 %

Show Material materials with Elongation of 7.0 %

T6

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Bar

A50

7.0 %

Show Material materials with Elongation of 7.0 %

T6

EN 573-3, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar

A100

8.0 %

Show Material materials with Elongation of 8.0 %

T6

EN 573-3, EN 754

Strip, Sheet, Plate, Forging, Tube, Bar

A100

20.0 °C

2.0 %

Show Material materials with Elongation of 2.0 %

T6

EN 573-3

Flat

Transverse

20.0 °C

2.0 %

Show Material materials with Elongation of 2.0 %

T6

EN 573-3

Sheet

20.0 °C

3.0 %

Show Material materials with Elongation of 3.0 %

T6

EN 573-3

Forging

Transverse

20.0 °C

3.0 %

Show Material materials with Elongation of 3.0 %

T6

EN 573-3

Forging

20.0 °C

4.0 %

Show Material materials with Elongation of 4.0 %

T6

EN 573-3

Flat

Transverse

20.0 °C

4.0 %

Show Material materials with Elongation of 4.0 %

T6

EN 573-3

Sheet, Flat

20.0 °C

4.0 %

Show Material materials with Elongation of 4.0 %

T6

EN 573-3

Tube

A50

20.0 °C

5.0 %

Show Material materials with Elongation of 5.0 %

T6

EN 573-3

Flat

Transverse

20.0 °C

5.0 %

Show Material materials with Elongation of 5.0 %

T6

EN 573-3

Rod, Sheet, Flat

20.0 °C

5.0 %

Show Material materials with Elongation of 5.0 %

T6

EN 573-3

Profile, Rod, Tube

A50

20.0 °C

6.0 %

Show Material materials with Elongation of 6.0 %

T6

EN 573-3

Flat

A50 Transverse

20.0 °C

6.0 %

Show Material materials with Elongation of 6.0 %

T6

EN 573-3

Flat

Transverse

20.0 °C

6.0 %

Show Material materials with Elongation of 6.0 %

T6

EN 573-3

Flat, Forging, Rod, Tube

20.0 °C

6.0 %

Show Material materials with Elongation of 6.0 %

T6

EN 573-3

Rod, Tube, Flat

A50

20.0 °C

7.0 %

Show Material materials with Elongation of 7.0 %

T6

EN 573-3

Flat

A50 Transverse

20.0 °C

7.0 %

Show Material materials with Elongation of 7.0 %

T6

EN 573-3

Profile, Rod, Tube

20.0 °C

7.0 %

Show Material materials with Elongation of 7.0 %

T6

EN 573-3

Flat

A50

20.0 °C

8.0 %

Show Material materials with Elongation of 8.0 %

T6

EN 573-3

Rod, Tube

20.0 °C

8.0 %

Show Material materials with Elongation of 8.0 %

T6

EN 573-3

Flat

A50

20.0 °C

13.0 %

Show Material materials with Elongation of 13.0 %

T6

EN 573-3

A50 Transverse

20.0 °C

16.0 %

Show Material materials with Elongation of 16.0 %

T6

EN 573-3

A50 Transverse

Hardness, Brinell

123.0 [-]

Show Material materials with Hardness, Brinell of 123.0 [-]

T6

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Bar

125.0 [-]

Show Material materials with Hardness, Brinell of 125.0 [-]

T6

EN 573-3, EN 586

Strip, Sheet, Plate, Forging, Tube, Bar

126.0 [-]

Show Material materials with Hardness, Brinell of 126.0 [-]

T6

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Bar

131.0 [-]

Show Material materials with Hardness, Brinell of 131.0 [-]

T6

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Bar

133.0 [-]

Show Material materials with Hardness, Brinell of 133.0 [-]

T6

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Bar

135.0 [-]

Show Material materials with Hardness, Brinell of 135.0 [-]

T6

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Bar

138.0 [-]

Show Material materials with Hardness, Brinell of 138.0 [-]

T6

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Bar

20.0 °C

123.0 - 133.0 [-]

Show Material materials with Hardness, Brinell of 123.0 - 133.0 [-]

T6

EN 573-3

Flat

20.0 °C

123.0 - 135.0 [-]

Show Material materials with Hardness, Brinell of 123.0 - 135.0 [-]

T6

EN 573-3

Flat, Sheet

20.0 °C

123.0 - 138.0 [-]

Show Material materials with Hardness, Brinell of 123.0 - 138.0 [-]

T6

EN 573-3

Flat

20.0 °C

123.0 - 131.0 [-]

Show Material materials with Hardness, Brinell of 123.0 - 131.0 [-]

T6

EN 573-3

Flat, Sheet

20.0 °C

123.0 - 126.0 [-]

Show Material materials with Hardness, Brinell of 123.0 - 126.0 [-]

T6

EN 573-3

Flat, Sheet

20.0 °C

123.0 [-]

Show Material materials with Hardness, Brinell of 123.0 [-]

T6

EN 573-3

Flat, Sheet

20.0 °C

125.0 [-]

Show Material materials with Hardness, Brinell of 125.0 [-]

T6

EN 573-3

Forging

20.0 °C

126.0 - 133.0 [-]

Show Material materials with Hardness, Brinell of 126.0 - 133.0 [-]

T6

EN 573-3

Flat

20.0 °C

126.0 - 135.0 [-]

Show Material materials with Hardness, Brinell of 126.0 - 135.0 [-]

T6

EN 573-3

Flat, Sheet

20.0 °C

126.0 - 138.0 [-]

Show Material materials with Hardness, Brinell of 126.0 - 138.0 [-]

T6

EN 573-3

Flat

20.0 °C

126.0 - 131.0 [-]

Show Material materials with Hardness, Brinell of 126.0 - 131.0 [-]

T6

EN 573-3

Flat, Sheet

20.0 °C

126.0 [-]

Show Material materials with Hardness, Brinell of 126.0 [-]

T6

EN 573-3

Flat, Sheet

20.0 °C

131.0 - 133.0 [-]

Show Material materials with Hardness, Brinell of 131.0 - 133.0 [-]

T6

EN 573-3

Flat

20.0 °C

131.0 - 135.0 [-]

Show Material materials with Hardness, Brinell of 131.0 - 135.0 [-]

T6

EN 573-3

Flat, Sheet

20.0 °C

131.0 - 138.0 [-]

Show Material materials with Hardness, Brinell of 131.0 - 138.0 [-]

T6

EN 573-3

Flat

20.0 °C

131.0 [-]

Show Material materials with Hardness, Brinell of 131.0 [-]

T6

EN 573-3

Flat, Sheet

20.0 °C

133.0 [-]

Show Material materials with Hardness, Brinell of 133.0 [-]

T6

EN 573-3

Flat

20.0 °C

133.0 - 135.0 [-]

Show Material materials with Hardness, Brinell of 133.0 - 135.0 [-]

T6

EN 573-3

Flat

20.0 °C

133.0 - 138.0 [-]

Show Material materials with Hardness, Brinell of 133.0 - 138.0 [-]

T6

EN 573-3

Flat

20.0 °C

135.0 [-]

Show Material materials with Hardness, Brinell of 135.0 [-]

T6

EN 573-3

Flat, Sheet

20.0 °C

135.0 - 138.0 [-]

Show Material materials with Hardness, Brinell of 135.0 - 138.0 [-]

T6

EN 573-3

Flat

20.0 °C

138.0 [-]

Show Material materials with Hardness, Brinell of 138.0 [-]

T6

EN 573-3

Flat

20.0 °C

140.0 [-]

Show Material materials with Hardness, Brinell of 140.0 [-]

T6

EN 573-3

Profile, Rod, Tube

20.0 °C

150.0 [-]

Show Material materials with Hardness, Brinell of 150.0 [-]

T6

EN 573-3

Flat

Plane-Strain Fracture Toughnes

20.0 °C

18.3 - 30.6 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 18.3 - 30.6 MPa·√m

T6

EN 573-3

20.0 °C

18.3 - 19.1 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 18.3 - 19.1 MPa·√m

T6

EN 573-3

20.0 °C

18.3 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 18.3 MPa·√m

T6

EN 573-3

20.0 °C

19.1 - 30.6 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 19.1 - 30.6 MPa·√m

T6

EN 573-3

20.0 °C

19.1 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 19.1 MPa·√m

T6

EN 573-3

20.0 °C

30.6 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 30.6 MPa·√m

T6

EN 573-3

Poisson's ratio

-269.0 °C

0.335 [-]

Show Material materials with Poisson's ratio of 0.335 [-]

T6

EN 573-3

-195.0 °C

0.337 [-]

Show Material materials with Poisson's ratio of 0.337 [-]

T6

EN 573-3

27.0 °C

0.321 [-]

Show Material materials with Poisson's ratio of 0.321 [-]

T6

EN 573-3

Shear modulus

27.4 GPa

Show Material materials with Shear modulus of 27.4 GPa

T6

EN 573-3, EN 485, EN 586, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar

Tensile strength

-269.0 °C

817.0 MPa

Show Material materials with Tensile strength of 817.0 MPa

T6

EN 573-3

-195.0 °C

593.6 MPa

Show Material materials with Tensile strength of 593.6 MPa

T6

EN 573-3

390.0 MPa

Show Material materials with Tensile strength of 390.0 MPa

T6

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Bar

410.0 MPa

Show Material materials with Tensile strength of 410.0 MPa

T6

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Bar

415.0 MPa

Show Material materials with Tensile strength of 415.0 MPa

T6

EN 573-3, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar

420.0 MPa

Show Material materials with Tensile strength of 420.0 MPa

T6

EN 573-3, EN 485, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar

430.0 MPa

Show Material materials with Tensile strength of 430.0 MPa

T6

EN 573-3, EN 586, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar

435.0 MPa

Show Material materials with Tensile strength of 435.0 MPa

T6

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Bar

440.0 MPa

Show Material materials with Tensile strength of 440.0 MPa

T6

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Bar

450.0 MPa

Show Material materials with Tensile strength of 450.0 MPa

T6

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar

460.0 MPa

Show Material materials with Tensile strength of 460.0 MPa

T6

EN 573-3, EN 485, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar

465.0 MPa

Show Material materials with Tensile strength of 465.0 MPa

T6

EN 573-3, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar

20.0 °C

220.0 MPa

Show Material materials with Tensile strength of 220.0 MPa

T6

EN 573-3

Transverse

20.0 °C

390.0 MPa

Show Material materials with Tensile strength of 390.0 MPa

T6

EN 573-3

Flat

Transverse

20.0 °C

390.0 MPa

Show Material materials with Tensile strength of 390.0 MPa

T6

EN 573-3

Sheet

20.0 °C

410.0 MPa

Show Material materials with Tensile strength of 410.0 MPa

T6

EN 573-3

Flat

Transverse

20.0 °C

410.0 MPa

Show Material materials with Tensile strength of 410.0 MPa

T6

EN 573-3

Sheet, Flat

20.0 °C

415.0 MPa

Show Material materials with Tensile strength of 415.0 MPa

T6

EN 573-3

Rod, Tube, Profile

20.0 °C

420.0 MPa

Show Material materials with Tensile strength of 420.0 MPa

T6

EN 573-3

Flat

Transverse

20.0 °C

420.0 MPa

Show Material materials with Tensile strength of 420.0 MPa

T6

EN 573-3

Rod, Sheet, Flat

20.0 °C

430.0 MPa

Show Material materials with Tensile strength of 430.0 MPa

T6

EN 573-3

Forging

Transverse

20.0 °C

430.0 MPa

Show Material materials with Tensile strength of 430.0 MPa

T6

EN 573-3

Rod, Forging, Flat

20.0 °C

435.0 MPa

Show Material materials with Tensile strength of 435.0 MPa

T6

EN 573-3

Flat

Transverse

20.0 °C

435.0 MPa

Show Material materials with Tensile strength of 435.0 MPa

T6

EN 573-3

Sheet

20.0 °C

440.0 MPa

Show Material materials with Tensile strength of 440.0 MPa

T6

EN 573-3

Flat

Transverse

20.0 °C

440.0 MPa

Show Material materials with Tensile strength of 440.0 MPa

T6

EN 573-3

Forging, Flat

20.0 °C

450.0 MPa

Show Material materials with Tensile strength of 450.0 MPa

T6

EN 573-3

Flat

Transverse

20.0 °C

450.0 MPa

Show Material materials with Tensile strength of 450.0 MPa

T6

EN 573-3

Rod, Tube, Sheet, Flat

20.0 °C

460.0 MPa

Show Material materials with Tensile strength of 460.0 MPa

T6

EN 573-3

Flat

Transverse

20.0 °C

460.0 MPa

Show Material materials with Tensile strength of 460.0 MPa

T6

EN 573-3

Rod, Profile, Flat

20.0 °C

465.0 MPa

Show Material materials with Tensile strength of 465.0 MPa

T6

EN 573-3

Rod

27.0 °C

534.3 MPa

Show Material materials with Tensile strength of 534.3 MPa

T6

EN 573-3

Yield strength

-269.0 °C

706.7 MPa

Show Material materials with Yield strength of 706.7 MPa

T6

EN 573-3

RP02

-195.0 °C

520.6 MPa

Show Material materials with Yield strength of 520.6 MPa

T6

EN 573-3

RP02

320.0 MPa

Show Material materials with Yield strength of 320.0 MPa

T6

EN 573-3, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar

RP02

340.0 MPa

Show Material materials with Yield strength of 340.0 MPa

T6

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Bar

RP02

350.0 MPa

Show Material materials with Yield strength of 350.0 MPa

T6

EN 573-3, EN 485, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar

RP02

360.0 MPa

Show Material materials with Yield strength of 360.0 MPa

T6

EN 573-3, EN 485, EN 586

Strip, Sheet, Plate, Forging, Tube, Bar

RP02

370.0 MPa

Show Material materials with Yield strength of 370.0 MPa

T6

EN 573-3, EN 586, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar

RP02

380.0 MPa

Show Material materials with Yield strength of 380.0 MPa

T6

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Forging, Tube, Bar

RP02

390.0 MPa

Show Material materials with Yield strength of 390.0 MPa

T6

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Bar

RP02

395.0 MPa

Show Material materials with Yield strength of 395.0 MPa

T6

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Bar

RP02

400.0 MPa

Show Material materials with Yield strength of 400.0 MPa

T6

EN 573-3, EN 485, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar

RP02

415.0 MPa

Show Material materials with Yield strength of 415.0 MPa

T6

EN 573-3, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar

RP02

420.0 MPa

Show Material materials with Yield strength of 420.0 MPa

T6

EN 573-3, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar

RP02

20.0 °C

25.0 MPa

Show Material materials with Yield strength of 25.0 MPa

T6

EN 573-3

Rod

RP02

20.0 °C

75.0 MPa

Show Material materials with Yield strength of 75.0 MPa

T6

EN 573-3

Rod

RP02

20.0 °C

140.0 MPa

Show Material materials with Yield strength of 140.0 MPa

T6

EN 573-3

RP02 Transverse

20.0 °C

150.0 MPa

Show Material materials with Yield strength of 150.0 MPa

T6

EN 573-3

Rod

RP02

20.0 °C

200.0 MPa

Show Material materials with Yield strength of 200.0 MPa

T6

EN 573-3

Rod

RP02

20.0 °C

250.0 MPa

Show Material materials with Yield strength of 250.0 MPa

T6

EN 573-3

Rod

RP02

20.0 °C

320.0 MPa

Show Material materials with Yield strength of 320.0 MPa

T6

EN 573-3

Rod

RP02

20.0 °C

340.0 MPa

Show Material materials with Yield strength of 340.0 MPa

T6

EN 573-3

Flat

RP02 Transverse

20.0 °C

340.0 MPa

Show Material materials with Yield strength of 340.0 MPa

T6

EN 573-3

Sheet

RP02

20.0 °C

350.0 MPa

Show Material materials with Yield strength of 350.0 MPa

T6

EN 573-3

Flat

RP02 Transverse

20.0 °C

350.0 MPa

Show Material materials with Yield strength of 350.0 MPa

T6

EN 573-3

Rod, Sheet, Flat

RP02

20.0 °C

360.0 MPa

Show Material materials with Yield strength of 360.0 MPa

T6

EN 573-3

Forging, Flat

RP02 Transverse

20.0 °C

360.0 MPa

Show Material materials with Yield strength of 360.0 MPa

T6

EN 573-3

Forging, Sheet

RP02

20.0 °C

360.0 - 385.0 MPa

Show Material materials with Yield strength of 360.0 - 385.0 MPa

T6

EN 573-3

20.0 °C

370.0 MPa

Show Material materials with Yield strength of 370.0 MPa

T6

EN 573-3

Forging

RP02 Transverse

20.0 °C

370.0 MPa

Show Material materials with Yield strength of 370.0 MPa

T6

EN 573-3

Rod, Tube, Forging, Profile, Flat

RP02

20.0 °C

380.0 MPa

Show Material materials with Yield strength of 380.0 MPa

T6

EN 573-3

Flat

RP02 Transverse

20.0 °C

380.0 MPa

Show Material materials with Yield strength of 380.0 MPa

T6

EN 573-3

Rod, Tube, Forging, Sheet, Flat

RP02

20.0 °C

390.0 MPa

Show Material materials with Yield strength of 390.0 MPa

T6

EN 573-3

Flat

RP02 Transverse

20.0 °C

390.0 MPa

Show Material materials with Yield strength of 390.0 MPa

T6

EN 573-3

Sheet, Flat

RP02

20.0 °C

395.0 MPa

Show Material materials with Yield strength of 395.0 MPa

T6

EN 573-3

Flat

RP02 Transverse

20.0 °C

395.0 MPa

Show Material materials with Yield strength of 395.0 MPa

T6

EN 573-3

Flat

RP02

20.0 °C

400.0 MPa

Show Material materials with Yield strength of 400.0 MPa

T6

EN 573-3

Flat

RP02 Transverse

20.0 °C

400.0 MPa

Show Material materials with Yield strength of 400.0 MPa

T6

EN 573-3

Tube, Flat

RP02

20.0 °C

410.0 MPa

Show Material materials with Yield strength of 410.0 MPa

T6

EN 573-3

Flat

RP02

20.0 °C

415.0 MPa

Show Material materials with Yield strength of 415.0 MPa

T6

EN 573-3

Rod, Profile

RP02

20.0 °C

420.0 MPa

Show Material materials with Yield strength of 420.0 MPa

T6

EN 573-3

Rod

RP02

27.0 °C

485.4 MPa

Show Material materials with Yield strength of 485.4 MPa

T6

EN 573-3

RP02

Thermal

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coefficient of thermal expansion

-50 °C

2.1e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.1e-05 1/K

T6

EN 573-3, EN 485, EN 586, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar, Profile, Rod, Flat

-50.0 °C

2.1e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.1e-05 1/K

T6

EN 573-3, EN 485, EN 586, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar, Profile, Rod, Flat

20 °C

2.1e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.1e-05 1/K

T6

EN 573-3, EN 485, EN 586, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar, Profile, Rod, Flat

20 °C

2.28e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.28e-05 1/K

T6

EN 573-3, EN 485, EN 586, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar, Profile, Rod, Flat

20 °C

2.3e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3e-05 1/K

T6

EN 573-3, EN 485, EN 586, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar

20 °C

2.36e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.36e-05 1/K

T6

EN 573-3, EN 485, EN 586, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar, Profile, Rod, Flat

20 °C

2.46e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.46e-05 1/K

T6

EN 573-3, EN 485, EN 586, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar, Profile, Rod, Flat

100 °C

2.28e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.28e-05 1/K

T6

EN 573-3, EN 485, EN 586, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar, Profile, Rod, Flat

100.0 °C

2.28e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.28e-05 1/K

T6

EN 573-3, EN 485, EN 586, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar, Profile, Rod, Flat

100 °C

2.3e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3e-05 1/K

T6

EN 573-3, EN 485, EN 586, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar

200 °C

2.36e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.36e-05 1/K

T6

EN 573-3, EN 485, EN 586, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar, Profile, Rod, Flat

200.0 °C

2.36e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.36e-05 1/K

T6

EN 573-3, EN 485, EN 586, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar, Profile, Rod, Flat

300 °C

2.46e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.46e-05 1/K

T6

EN 573-3, EN 485, EN 586, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar, Profile, Rod, Flat

300.0 °C

2.46e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.46e-05 1/K

T6

EN 573-3, EN 485, EN 586, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar, Profile, Rod, Flat

Melting point

505.0 - 635.0 °C

Show Material materials with Melting point of 505.0 - 635.0 °C

T6

EN 573-3, EN 485, EN 586, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar

510.0 - 640.0 °C

Show Material materials with Melting point of 510.0 - 640.0 °C

T6

EN 573-3, EN 485, EN 586, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar

Specific heat capacity

816.0 - 963.0 J/(kg·K)

Show Material materials with Specific heat capacity of 816.0 - 963.0 J/(kg·K)

Typical for Wrought 2000 Series Aluminium

Thermal conductivity

134.0 - 193.0 W/(m·K)

Show Material materials with Thermal conductivity of 134.0 - 193.0 W/(m·K)

T6

EN 573-3, EN 485, EN 586, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar

20.0 °C

140.0 - 200.0 W/(m·K)

Show Material materials with Thermal conductivity of 140.0 - 200.0 W/(m·K)

T6

EN 573-3, EN 485, EN 586, EN 754, EN 755

Forging, Profile, Rod, Flat, Tube, Sheet, Strip, Plate, Bar

Electrical

PropertyTemperatureValueConditionRelated StandardsShape

Electrical conductivity

21000000.0 - 24000000.0 S/m

Show Material materials with Electrical conductivity of 21000000.0 - 24000000.0 S/m

T6

EN 573-3, EN 485, EN 586, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar

20.0 °C

20000000.0 - 29000000.0 S/m

Show Material materials with Electrical conductivity of 20000000.0 - 29000000.0 S/m

T6

EN 573-3, EN 485, EN 586, EN 754, EN 755

Forging, Profile, Rod, Flat, Tube, Sheet, Strip, Plate, Bar

Electrical resistivity

3.45e-08 - 5e-08 Ω·m

Show Material materials with Electrical resistivity of 3.45e-08 - 5e-08 Ω·m

T6

EN 573-3, EN 485, EN 586, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar

4.17e-08 - 4.76e-08 Ω·m

Show Material materials with Electrical resistivity of 4.17e-08 - 4.76e-08 Ω·m

T6

EN 573-3, EN 485, EN 586, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar

Chemical properties

PropertyValueConditionRelated StandardsShape

Chromium

0.1 %

Show Material materials with Chromium of 0.1 %

T6

EN 573-3, EN 485, EN 586, EN 754, EN 755

Forging, Profile, Rod, Flat, Tube, Sheet, Strip, Plate, Bar

Copper

3.9 - 5.0 %

Show Material materials with Copper of 3.9 - 5.0 %

T6

EN 573-3, EN 485, EN 586, EN 754, EN 755

Forging, Profile, Rod, Flat, Tube, Sheet, Strip, Plate, Bar

Iron

0.5 %

Show Material materials with Iron of 0.5 %

T6

EN 573-3

Profile, Rod, Flat, Tube

0.7 %

Show Material materials with Iron of 0.7 %

T6

EN 573-3

Forging, Profile, Rod, Flat, Tube, Sheet

0.70 %

Show Material materials with Iron of 0.70 %

T6

EN 573-3, EN 485, EN 586, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Bar

Magnesium

0.2 - 0.8 %

Show Material materials with Magnesium of 0.2 - 0.8 %

T6

EN 573-3, EN 485, EN 586, EN 754, EN 755

Forging, Profile, Rod, Flat, Tube, Sheet, Strip, Plate, Bar

Manganese

0.4 - 1.2 %

Show Material materials with Manganese of 0.4 - 1.2 %

T6

EN 573-3, EN 485, EN 586, EN 754, EN 755

Forging, Profile, Rod, Flat, Tube, Sheet, Strip, Plate, Bar

Nickel

0.1

Show Material materials with Nickel of 0.1

T6

EN 573-3

Profile, Rod, Flat, Tube

Silicon

0.5 - 1.2 %

Show Material materials with Silicon of 0.5 - 1.2 %

T6

EN 573-3, EN 485, EN 586, EN 754, EN 755

Forging, Profile, Rod, Flat, Tube, Sheet, Strip, Plate, Bar

0.5 - 0.9 %

Show Material materials with Silicon of 0.5 - 0.9 %

T6

EN 573-3

Profile, Rod, Flat, Tube

Titanium

0.15 %

Show Material materials with Titanium of 0.15 %

T6

EN 573-3, EN 485, EN 586, EN 754, EN 755

Forging, Profile, Rod, Flat, Tube, Sheet, Strip, Plate, Bar

Zinc

0.25 %

Show Material materials with Zinc of 0.25 %

T6

EN 573-3, EN 485, EN 586, EN 754, EN 755

Forging, Profile, Rod, Flat, Tube, Sheet, Strip, Plate, Bar

Technological properties

Property
Anodizing

decorative: not suitable, Protective: acceptable

Brazing

hard brazing (with flux/ without flux): not suitable / not suitable, friction soldering: acceptable, soft brazing with flux: not suitable

Corrosion properties

Seawater: sufficient, weathering: acceptable

Workability

Bending / Spinning (cold): gut (O) / ungeeignet, Impact extrusion (cold): not suitable, Deep drawing / upsetting (Condition) acceptable (O) / not suitable