Hardenable austenitic high temperature special steel with resistance to scaling up to 750 °C and high temperature strength up to 650 °C. Application: steam vessel and turbine manufacturing, in the chemicals industry and petrochemistry, for power plant pipes and in the hardened condition for blades, spindles, screws in the power plant engineering

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

7.96 g/cm³

Show Material materials with Density of 7.96 g/cm³

50.0 °C

7.95 g/cm³

Show Material materials with Density of 7.95 g/cm³

100.0 °C

7.93 g/cm³

Show Material materials with Density of 7.93 g/cm³

150.0 °C

7.9 g/cm³

Show Material materials with Density of 7.9 g/cm³

200.0 °C

7.88 g/cm³

Show Material materials with Density of 7.88 g/cm³

250.0 °C

7.86 g/cm³

Show Material materials with Density of 7.86 g/cm³

300.0 °C

7.84 g/cm³

Show Material materials with Density of 7.84 g/cm³

350.0 °C

7.82 g/cm³

Show Material materials with Density of 7.82 g/cm³

400.0 °C

7.79 g/cm³

Show Material materials with Density of 7.79 g/cm³

450.0 °C

7.77 g/cm³

Show Material materials with Density of 7.77 g/cm³

500.0 °C

7.75 g/cm³

Show Material materials with Density of 7.75 g/cm³

550.0 °C

7.72 g/cm³

Show Material materials with Density of 7.72 g/cm³

600.0 °C

7.7 g/cm³

Show Material materials with Density of 7.7 g/cm³

650.0 °C

7.67 g/cm³

Show Material materials with Density of 7.67 g/cm³

700.0 °C

7.65 g/cm³

Show Material materials with Density of 7.65 g/cm³

750.0 °C

7.62 g/cm³

Show Material materials with Density of 7.62 g/cm³

800.0 °C

7.6 g/cm³

Show Material materials with Density of 7.6 g/cm³

Mechanical

PropertyTemperatureValue

Elastic modulus

-100.0 °C

206 GPa

Show Material materials with Elastic modulus of 206 GPa

20.0 °C

196 - 198 GPa

Show Material materials with Elastic modulus of 196 - 198 GPa

50.0 °C

194.83 GPa

Show Material materials with Elastic modulus of 194.83 GPa

100.0 °C

190 - 192 GPa

Show Material materials with Elastic modulus of 190 - 192 GPa

150.0 °C

186.88 GPa

Show Material materials with Elastic modulus of 186.88 GPa

200.0 °C

182 - 183 GPa

Show Material materials with Elastic modulus of 182 - 183 GPa

250.0 °C

178.44 GPa

Show Material materials with Elastic modulus of 178.44 GPa

300.0 °C

174 - 175 GPa

Show Material materials with Elastic modulus of 174 - 175 GPa

350.0 °C

169.81 GPa

Show Material materials with Elastic modulus of 169.81 GPa

400.0 °C

165.69 - 167 GPa

Show Material materials with Elastic modulus of 165.69 - 167 GPa

450.0 °C

161.57 GPa

Show Material materials with Elastic modulus of 161.57 GPa

500.0 °C

157.45 - 159 GPa

Show Material materials with Elastic modulus of 157.45 - 159 GPa

550.0 °C

153.43 GPa

Show Material materials with Elastic modulus of 153.43 GPa

600.0 °C

149.5 - 150 GPa

Show Material materials with Elastic modulus of 149.5 - 150 GPa

650.0 °C

145.58 GPa

Show Material materials with Elastic modulus of 145.58 GPa

700.0 °C

141.66 - 142 GPa

Show Material materials with Elastic modulus of 141.66 - 142 GPa

750.0 °C

138.03 GPa

Show Material materials with Elastic modulus of 138.03 GPa

800.0 °C

134 - 134.3 GPa

Show Material materials with Elastic modulus of 134 - 134.3 GPa

900.0 °C

127 GPa

Show Material materials with Elastic modulus of 127 GPa

1000.0 °C

120 GPa

Show Material materials with Elastic modulus of 120 GPa

Unlock all property charts

Elongation

20.0 °C

20 - 30 %

Show Material materials with Elongation of 20 - 30 %

Poisson's ratio

20.0 °C

0.28 [-]

Show Material materials with Poisson's ratio of 0.28 [-]

50.0 °C

0.28 [-]

Show Material materials with Poisson's ratio of 0.28 [-]

100.0 °C

0.28 [-]

Show Material materials with Poisson's ratio of 0.28 [-]

150.0 °C

0.28 [-]

Show Material materials with Poisson's ratio of 0.28 [-]

200.0 °C

0.29 [-]

Show Material materials with Poisson's ratio of 0.29 [-]

250.0 °C

0.29 [-]

Show Material materials with Poisson's ratio of 0.29 [-]

300.0 °C

0.29 [-]

Show Material materials with Poisson's ratio of 0.29 [-]

350.0 °C

0.29 [-]

Show Material materials with Poisson's ratio of 0.29 [-]

400.0 °C

0.3 [-]

Show Material materials with Poisson's ratio of 0.3 [-]

450.0 °C

0.3 [-]

Show Material materials with Poisson's ratio of 0.3 [-]

500.0 °C

0.3 [-]

Show Material materials with Poisson's ratio of 0.3 [-]

550.0 °C

0.31 [-]

Show Material materials with Poisson's ratio of 0.31 [-]

600.0 °C

0.31 [-]

Show Material materials with Poisson's ratio of 0.31 [-]

650.0 °C

0.31 [-]

Show Material materials with Poisson's ratio of 0.31 [-]

700.0 °C

0.32 [-]

Show Material materials with Poisson's ratio of 0.32 [-]

750.0 °C

0.32 [-]

Show Material materials with Poisson's ratio of 0.32 [-]

800.0 °C

0.32 [-]

Show Material materials with Poisson's ratio of 0.32 [-]

Unlock all property charts

Shear modulus

20.0 °C

77.01 GPa

Show Material materials with Shear modulus of 77.01 GPa

50.0 °C

76.13 GPa

Show Material materials with Shear modulus of 76.13 GPa

100.0 °C

74.56 GPa

Show Material materials with Shear modulus of 74.56 GPa

150.0 °C

72.79 GPa

Show Material materials with Shear modulus of 72.79 GPa

200.0 °C

71.02 GPa

Show Material materials with Shear modulus of 71.02 GPa

250.0 °C

69.26 GPa

Show Material materials with Shear modulus of 69.26 GPa

300.0 °C

67.39 GPa

Show Material materials with Shear modulus of 67.39 GPa

350.0 °C

65.63 GPa

Show Material materials with Shear modulus of 65.63 GPa

400.0 °C

63.86 GPa

Show Material materials with Shear modulus of 63.86 GPa

450.0 °C

62.1 GPa

Show Material materials with Shear modulus of 62.1 GPa

500.0 °C

60.43 GPa

Show Material materials with Shear modulus of 60.43 GPa

550.0 °C

58.76 GPa

Show Material materials with Shear modulus of 58.76 GPa

600.0 °C

57.09 GPa

Show Material materials with Shear modulus of 57.09 GPa

650.0 °C

55.43 GPa

Show Material materials with Shear modulus of 55.43 GPa

700.0 °C

53.86 GPa

Show Material materials with Shear modulus of 53.86 GPa

750.0 °C

52.29 GPa

Show Material materials with Shear modulus of 52.29 GPa

800.0 °C

50.72 GPa

Show Material materials with Shear modulus of 50.72 GPa

Unlock all property charts

Tensile strength

20.0 °C

540 - 740 MPa

Show Material materials with Tensile strength of 540 - 740 MPa

Yield strength Rp0.2

20.0 °C

225 MPa

Show Material materials with Yield strength Rp0.2 of 225 MPa

100.0 °C

215 MPa

Show Material materials with Yield strength Rp0.2 of 215 MPa

200.0 °C

196 MPa

Show Material materials with Yield strength Rp0.2 of 196 MPa

300.0 °C

177 MPa

Show Material materials with Yield strength Rp0.2 of 177 MPa

400.0 °C

167 MPa

Show Material materials with Yield strength Rp0.2 of 167 MPa

500.0 °C

157 MPa

Show Material materials with Yield strength Rp0.2 of 157 MPa

550.0 °C

152 MPa

Show Material materials with Yield strength Rp0.2 of 152 MPa

600.0 °C

147 MPa

Show Material materials with Yield strength Rp0.2 of 147 MPa

Unlock all property charts

Yield strength Rp1.0

20.0 °C

295 MPa

Show Material materials with Yield strength Rp1.0 of 295 MPa

100.0 °C

245 MPa

Show Material materials with Yield strength Rp1.0 of 245 MPa

200.0 °C

226 MPa

Show Material materials with Yield strength Rp1.0 of 226 MPa

300.0 °C

206 MPa

Show Material materials with Yield strength Rp1.0 of 206 MPa

400.0 °C

196 MPa

Show Material materials with Yield strength Rp1.0 of 196 MPa

500.0 °C

186 MPa

Show Material materials with Yield strength Rp1.0 of 186 MPa

550.0 °C

181 MPa

Show Material materials with Yield strength Rp1.0 of 181 MPa

600.0 °C

177 MPa

Show Material materials with Yield strength Rp1.0 of 177 MPa

Unlock all property charts

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

-100.0 °C

1.49E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.49E-5 1/K

20.0 °C

1.61E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.61E-5 1/K

100.0 °C

1.63E-5 - 1.67E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.63E-5 - 1.67E-5 1/K

200.0 °C

1.68E-5 - 1.72E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.68E-5 - 1.72E-5 1/K

300.0 °C

1.73E-5 - 1.77E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.73E-5 - 1.77E-5 1/K

400.0 °C

1.78E-5 - 1.81E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.78E-5 - 1.81E-5 1/K

500.0 °C

1.82E-5 - 1.84E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.82E-5 - 1.84E-5 1/K

600.0 °C

1.85E-5 - 1.88E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.85E-5 - 1.88E-5 1/K

700.0 °C

1.87E-5 - 1.91E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.87E-5 - 1.91E-5 1/K

800.0 °C

1.94E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.94E-5 1/K

900.0 °C

1.97E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.97E-5 1/K

1000.0 °C

2E-5 1/K

Show Material materials with Coefficient of thermal expansion of 2E-5 1/K

Unlock all property charts

Max service temperature, long

0 - 750 °C

Show Material materials with Max service temperature, long of 0 - 750 °C

Melting point

1230 - 1480 °C

Show Material materials with Melting point of 1230 - 1480 °C

Typical for Austenitic Stainless Steel

Specific heat capacity

-100.0 °C

440 J/(kg·K)

Show Material materials with Specific heat capacity of 440 J/(kg·K)

20.0 °C

450 - 472 J/(kg·K)

Show Material materials with Specific heat capacity of 450 - 472 J/(kg·K)

100.0 °C

487 J/(kg·K)

Show Material materials with Specific heat capacity of 487 J/(kg·K)

200.0 °C

503 J/(kg·K)

Show Material materials with Specific heat capacity of 503 J/(kg·K)

300.0 °C

512 J/(kg·K)

Show Material materials with Specific heat capacity of 512 J/(kg·K)

400.0 °C

520 J/(kg·K)

Show Material materials with Specific heat capacity of 520 J/(kg·K)

500.0 °C

530 J/(kg·K)

Show Material materials with Specific heat capacity of 530 J/(kg·K)

600.0 °C

541 J/(kg·K)

Show Material materials with Specific heat capacity of 541 J/(kg·K)

700.0 °C

551 J/(kg·K)

Show Material materials with Specific heat capacity of 551 J/(kg·K)

800.0 °C

559 J/(kg·K)

Show Material materials with Specific heat capacity of 559 J/(kg·K)

900.0 °C

565 J/(kg·K)

Show Material materials with Specific heat capacity of 565 J/(kg·K)

1000.0 °C

571 J/(kg·K)

Show Material materials with Specific heat capacity of 571 J/(kg·K)

Unlock all property charts

Thermal conductivity

20.0 °C

13.3 - 15 W/(m·K)

Show Material materials with Thermal conductivity of 13.3 - 15 W/(m·K)

100.0 °C

14.9 W/(m·K)

Show Material materials with Thermal conductivity of 14.9 W/(m·K)

200.0 °C

16.5 W/(m·K)

Show Material materials with Thermal conductivity of 16.5 W/(m·K)

300.0 °C

18.1 W/(m·K)

Show Material materials with Thermal conductivity of 18.1 W/(m·K)

400.0 °C

19.5 W/(m·K)

Show Material materials with Thermal conductivity of 19.5 W/(m·K)

500.0 °C

21 W/(m·K)

Show Material materials with Thermal conductivity of 21 W/(m·K)

600.0 °C

22.4 W/(m·K)

Show Material materials with Thermal conductivity of 22.4 W/(m·K)

700.0 °C

23.8 W/(m·K)

Show Material materials with Thermal conductivity of 23.8 W/(m·K)

800.0 °C

25.2 W/(m·K)

Show Material materials with Thermal conductivity of 25.2 W/(m·K)

Unlock all property charts

Thermal diffusivity

20.0 °C

3.5 mm²/s

Show Material materials with Thermal diffusivity of 3.5 mm²/s

100.0 °C

3.8 mm²/s

Show Material materials with Thermal diffusivity of 3.8 mm²/s

200.0 °C

4 mm²/s

Show Material materials with Thermal diffusivity of 4 mm²/s

300.0 °C

4.3 mm²/s

Show Material materials with Thermal diffusivity of 4.3 mm²/s

400.0 °C

4.5 mm²/s

Show Material materials with Thermal diffusivity of 4.5 mm²/s

500.0 °C

4.7 mm²/s

Show Material materials with Thermal diffusivity of 4.7 mm²/s

600.0 °C

4.8 mm²/s

Show Material materials with Thermal diffusivity of 4.8 mm²/s

700.0 °C

5.1 mm²/s

Show Material materials with Thermal diffusivity of 5.1 mm²/s

800.0 °C

5.4 mm²/s

Show Material materials with Thermal diffusivity of 5.4 mm²/s

Unlock all property charts

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

7.9E-7 - 7.91E-7 Ω·m

Show Material materials with Electrical resistivity of 7.9E-7 - 7.91E-7 Ω·m

50.0 °C

8.13E-7 Ω·m

Show Material materials with Electrical resistivity of 8.13E-7 Ω·m

100.0 °C

8.45E-7 Ω·m

Show Material materials with Electrical resistivity of 8.45E-7 Ω·m

150.0 °C

8.87E-7 Ω·m

Show Material materials with Electrical resistivity of 8.87E-7 Ω·m

200.0 °C

9.19E-7 Ω·m

Show Material materials with Electrical resistivity of 9.19E-7 Ω·m

250.0 °C

9.46E-7 Ω·m

Show Material materials with Electrical resistivity of 9.46E-7 Ω·m

300.0 °C

9.77E-7 Ω·m

Show Material materials with Electrical resistivity of 9.77E-7 Ω·m

350.0 °C

1E-6 Ω·m

Show Material materials with Electrical resistivity of 1E-6 Ω·m

400.0 °C

1.03E-6 Ω·m

Show Material materials with Electrical resistivity of 1.03E-6 Ω·m

450.0 °C

1.05E-6 Ω·m

Show Material materials with Electrical resistivity of 1.05E-6 Ω·m

500.0 °C

1.08E-6 Ω·m

Show Material materials with Electrical resistivity of 1.08E-6 Ω·m

550.0 °C

1.1E-6 Ω·m

Show Material materials with Electrical resistivity of 1.1E-6 Ω·m

600.0 °C

1.12E-6 Ω·m

Show Material materials with Electrical resistivity of 1.12E-6 Ω·m

650.0 °C

1.13E-6 Ω·m

Show Material materials with Electrical resistivity of 1.13E-6 Ω·m

700.0 °C

1.15E-6 Ω·m

Show Material materials with Electrical resistivity of 1.15E-6 Ω·m

750.0 °C

1.17E-6 Ω·m

Show Material materials with Electrical resistivity of 1.17E-6 Ω·m

800.0 °C

1.18E-6 Ω·m

Show Material materials with Electrical resistivity of 1.18E-6 Ω·m

Unlock all property charts

Chemical properties

PropertyValue

Carbon

0.04 - 0.1 %

Show Material materials with Carbon of 0.04 - 0.1 %

Chromium

15.5 - 17.5 %

Show Material materials with Chromium of 15.5 - 17.5 %

Manganese

1.5 %

Show Material materials with Manganese of 1.5 %

Molybdenum

1.1 - 1.5 %

Show Material materials with Molybdenum of 1.1 - 1.5 %

Nickel

12.5 - 14.5 %

Show Material materials with Nickel of 12.5 - 14.5 %

Nitrogen

0.06 - 0.14 %

Show Material materials with Nitrogen of 0.06 - 0.14 %

Phosphorus

0.04 %

Show Material materials with Phosphorus of 0.04 %

Silicon

0.3 - 0.6 %

Show Material materials with Silicon of 0.3 - 0.6 %

Sulfur

0.015 %

Show Material materials with Sulfur of 0.015 %

Vanadium

0.6 - 0.85 %