Description

Excellent corrosion resistance, electrical and thermal conductivity. High ductility and reflectivity. Anodizing quality. Brightness.

Related Standards

Equivalent Materials

Ashby charts

See where EN 573-1 Grade AW-1050A H24 falls on the material property chart for Density against Elastic modulus in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

Density

ρ

2.69 - 2.7 g/cm³ at 20 °C

Dimension

Dimensions

Dicke

Thickness

t

0.2 - 3 mm

Mechanical

Plane-Strain Fracture Toughnes

KIC

Typical for Wrought 1000 Series Aluminium

Tensile strength, transverse

Rm,trans

Yield strength Rp0.2, transverse

Rp0.2,trans

Thermal

Coefficient of thermal expansion

α

2.17E-5 1/K at -50 °C

20-100°C

Unlock all property charts

Melting point

Tm

646 - 657 °C

Specific heat capacity

cp

899 - 900 J/(kg·K) at 20 °C

Thermal conductivity

λ

138 - 229 W/(m·K) at 20 °C

Electrical

Electrical conductivity

σel

3.40E+7 - 3.60E+7 S/m at 20 °C

Electrical resistivity

ρel

2.78E-8 - 4.9E-8 Ω·m at 20 °C

Chemical properties

Element

Weight %

Comment

Al

99.5 %

Fe

0.4 %

Si

0.1 - 0.25 %

B

0.05 %

Cu

0.05 %

More

Technological properties

Anodizing

Excellent

Application areas

Facades: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Roofing: Single sheet, Sheets for composites/ sandwich Panels, Foil for bituminous coating; Doors: Sheets for mechanized panels; Sun Protection Systems: Single sheet (covering, sun breakers and gutters); Interiors and ceilings: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels, Decoration; Furniture, Plinths, Blinds: Single sheet, Intermediate transformation/interior use; Lighting: Anodizing Quality, Lacquering quality; Electronic devices: Housing of devices; Lithography; Cable Wrapping: Electric cable wrapping; Tubes: Industrial tubes, Flexible tube, Pipes; Insulation; Solar: Solar collectors, Photovoltaic panels; Wind energy: Nacelle coverings, rotor hub, stairs; Cosmetics: Cosmetics pieces; Automotive Trim: Interior Trim, Marque Badges; Components: Heat shields, General Transportation

Brazing

Excellent

Corrosion properties

Excellent

Welding

Excellent

Workability

Excellent

This material data has been provided by Aludium,WIAM,AluKey.