General
Property | Temperature | Value |
---|---|---|
Density | 20.0 °C | 7.85 g/cm³ Show Material materials with Density of 7.85 g/cm³ |
Mechanical
Property | Temperature | Value | Comment |
---|---|---|---|
Elastic modulus | 20.0 °C | 210 GPa Show Material materials with Elastic modulus of 210 GPa | |
200.0 °C | 193 GPa Show Material materials with Elastic modulus of 193 GPa | ||
300.0 °C | 185 GPa Show Material materials with Elastic modulus of 185 GPa | ||
400.0 °C | 175 GPa Show Material materials with Elastic modulus of 175 GPa | ||
Elongation | 20.0 °C | 7 - 11 % Show Material materials with Elongation of 7 - 11 % | |
Poisson's ratio | 23.0 °C | 0.29 [-] Show Material materials with Poisson's ratio of 0.29 [-] | Typical for High Carbon Steel |
Shear modulus | 20.0 °C | 81 GPa Show Material materials with Shear modulus of 81 GPa | |
Tensile strength | 20.0 °C | 740 - 980 MPa Show Material materials with Tensile strength of 740 - 980 MPa | |
Yield strength | 20.0 °C | 450 - 570 MPa Show Material materials with Yield strength of 450 - 570 MPa |
Thermal
Property | Temperature | Value | Comment |
---|---|---|---|
Coefficient of thermal expansion | 100.0 °C | 1.1E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.1E-5 1/K | |
200.0 °C | 1.18E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.18E-5 1/K | ||
400.0 °C | 1.32E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.32E-5 1/K | ||
Max service temperature | 500 °C Show Material materials with Max service temperature of 500 °C | Typical for Carbon Steel | |
Melting point | 1289 - 1478 °C Show Material materials with Melting point of 1289 - 1478 °C | Typical for High Carbon Steel | |
Specific heat capacity | 100.0 °C | 500 J/(kg·K) Show Material materials with Specific heat capacity of 500 J/(kg·K) | |
200.0 °C | 540 J/(kg·K) Show Material materials with Specific heat capacity of 540 J/(kg·K) | ||
400.0 °C | 600 J/(kg·K) Show Material materials with Specific heat capacity of 600 J/(kg·K) | ||
Thermal conductivity | 20.0 °C | 46.5 W/(m·K) Show Material materials with Thermal conductivity of 46.5 W/(m·K) |
Electrical
Property | Temperature | Value |
---|---|---|
Electrical resistivity | 20.0 °C | 1.3E-7 Ω·m Show Material materials with Electrical resistivity of 1.3E-7 Ω·m |
Chemical properties
Property | Value |
---|---|
Carbon | 0.57 - 0.65 % Show Material materials with Carbon of 0.57 - 0.65 % |
Lead | 0.15 - 0.35 % Show Material materials with Lead of 0.15 - 0.35 % |
Manganese | 0.7 - 1.1 % Show Material materials with Manganese of 0.7 - 1.1 % |
Phosphorus | 0.06 % Show Material materials with Phosphorus of 0.06 % |
Silicon | 0.1 - 0.3 % Show Material materials with Silicon of 0.1 - 0.3 % |
Sulfur | 0.18 - 0.25 % Show Material materials with Sulfur of 0.18 - 0.25 % |