General
Property | Temperature | Value |
---|---|---|
Density | 20.0 °C | 7.82 - 7.85 g/cm³ Show Material materials with Density of 7.82 - 7.85 g/cm³ |
Mechanical
Property | Temperature | Value | Comment |
---|---|---|---|
Elastic modulus | -100.0 °C | 217 GPa Show Material materials with Elastic modulus of 217 GPa | |
20.0 °C | 210 - 212 GPa Show Material materials with Elastic modulus of 210 - 212 GPa | ||
100.0 °C | 205 - 207 GPa Show Material materials with Elastic modulus of 205 - 207 GPa | ||
200.0 °C | 195 - 199 GPa Show Material materials with Elastic modulus of 195 - 199 GPa | ||
300.0 °C | 185 - 192 GPa Show Material materials with Elastic modulus of 185 - 192 GPa | ||
400.0 °C | 175 - 184 GPa Show Material materials with Elastic modulus of 175 - 184 GPa | ||
500.0 °C | 175 GPa Show Material materials with Elastic modulus of 175 GPa | ||
600.0 °C | 164 GPa Show Material materials with Elastic modulus of 164 GPa | ||
Elongation | 20.0 °C | 17 - 20 % Show Material materials with Elongation of 17 - 20 % | |
Elongation, transverse | 20.0 °C | 15 - 18 % Show Material materials with Elongation, transverse of 15 - 18 % | |
Poisson's ratio | 23.0 °C | 0.29 [-] Show Material materials with Poisson's ratio of 0.29 [-] | Typical for Medium Carbon Steel |
Reduction of area | 20.0 °C | 40 - 50 % Show Material materials with Reduction of area of 40 - 50 % | |
Reduction of area, transverse | 20.0 °C | 40 - 50 % Show Material materials with Reduction of area, transverse of 40 - 50 % | |
Shear modulus | 20.0 °C | 81 GPa Show Material materials with Shear modulus of 81 GPa | |
Tensile strength | 20.0 °C | 500 - 830 MPa Show Material materials with Tensile strength of 500 - 830 MPa | |
Tensile strength, transverse | 20.0 °C | 500 - 830 MPa Show Material materials with Tensile strength, transverse of 500 - 830 MPa | |
Yield strength | 20.0 °C | 290 - 430 MPa Show Material materials with Yield strength of 290 - 430 MPa | |
Yield strength, transverse | 20.0 °C | 290 - 430 MPa Show Material materials with Yield strength, transverse of 290 - 430 MPa |
Thermal
Property | Temperature | Value | Comment |
---|---|---|---|
Coefficient of thermal expansion | -100.0 °C | 1.08E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.08E-5 1/K | |
20.0 °C | 1.19E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.19E-5 1/K | ||
100.0 °C | 1.11E-5 - 1.25E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.11E-5 - 1.25E-5 1/K | ||
200.0 °C | 1.21E-5 - 1.3E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.21E-5 - 1.3E-5 1/K | ||
300.0 °C | 1.29E-5 - 1.36E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.29E-5 - 1.36E-5 1/K | ||
400.0 °C | 1.35E-5 - 1.41E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.35E-5 - 1.41E-5 1/K | ||
500.0 °C | 1.45E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.45E-5 1/K | ||
600.0 °C | 1.49E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.49E-5 1/K | ||
Max service temperature | 500 °C Show Material materials with Max service temperature of 500 °C | Typical for Carbon Steel | |
Melting point | 1380 - 1514 °C Show Material materials with Melting point of 1380 - 1514 °C | Typical for Medium Carbon Steel | |
Specific heat capacity | -100.0 °C | 423 J/(kg·K) Show Material materials with Specific heat capacity of 423 J/(kg·K) | |
20.0 °C | 460 - 461 J/(kg·K) Show Material materials with Specific heat capacity of 460 - 461 J/(kg·K) | ||
100.0 °C | 479 J/(kg·K) Show Material materials with Specific heat capacity of 479 J/(kg·K) | ||
200.0 °C | 499 J/(kg·K) Show Material materials with Specific heat capacity of 499 J/(kg·K) | ||
300.0 °C | 517 J/(kg·K) Show Material materials with Specific heat capacity of 517 J/(kg·K) | ||
400.0 °C | 536 J/(kg·K) Show Material materials with Specific heat capacity of 536 J/(kg·K) | ||
500.0 °C | 558 J/(kg·K) Show Material materials with Specific heat capacity of 558 J/(kg·K) | ||
600.0 °C | 587 J/(kg·K) Show Material materials with Specific heat capacity of 587 J/(kg·K) | ||
Thermal conductivity | 20.0 °C | 48 - 50 W/(m·K) Show Material materials with Thermal conductivity of 48 - 50 W/(m·K) | |
100.0 °C | 48.9 - 51 W/(m·K) Show Material materials with Thermal conductivity of 48.9 - 51 W/(m·K) | ||
200.0 °C | 47.5 - 48.2 W/(m·K) Show Material materials with Thermal conductivity of 47.5 - 48.2 W/(m·K) | ||
300.0 °C | 44.7 - 45.6 W/(m·K) Show Material materials with Thermal conductivity of 44.7 - 45.6 W/(m·K) | ||
400.0 °C | 41.6 W/(m·K) Show Material materials with Thermal conductivity of 41.6 W/(m·K) | ||
500.0 °C | 38.6 W/(m·K) Show Material materials with Thermal conductivity of 38.6 W/(m·K) | ||
600.0 °C | 35.5 W/(m·K) Show Material materials with Thermal conductivity of 35.5 W/(m·K) | ||
Thermal diffusivity | 20.0 °C | 13.3 mm²/s Show Material materials with Thermal diffusivity of 13.3 mm²/s | |
100.0 °C | 12.6 mm²/s Show Material materials with Thermal diffusivity of 12.6 mm²/s | ||
200.0 °C | 11.5 mm²/s Show Material materials with Thermal diffusivity of 11.5 mm²/s | ||
300.0 °C | 10.2 mm²/s Show Material materials with Thermal diffusivity of 10.2 mm²/s | ||
400.0 °C | 8.9 mm²/s Show Material materials with Thermal diffusivity of 8.9 mm²/s | ||
500.0 °C | 7.5 mm²/s Show Material materials with Thermal diffusivity of 7.5 mm²/s | ||
600.0 °C | 6 mm²/s Show Material materials with Thermal diffusivity of 6 mm²/s | ||
Electrical
Property | Temperature | Value |
---|---|---|
Electrical resistivity | 20.0 °C | 1.2E-7 - 2.17E-7 Ω·m Show Material materials with Electrical resistivity of 1.2E-7 - 2.17E-7 Ω·m |
100.0 °C | 2.62E-7 Ω·m Show Material materials with Electrical resistivity of 2.62E-7 Ω·m | |
200.0 °C | 3.32E-7 Ω·m Show Material materials with Electrical resistivity of 3.32E-7 Ω·m | |
300.0 °C | 4.2E-7 Ω·m Show Material materials with Electrical resistivity of 4.2E-7 Ω·m | |
400.0 °C | 5.23E-7 Ω·m Show Material materials with Electrical resistivity of 5.23E-7 Ω·m | |
500.0 °C | 6.41E-7 Ω·m Show Material materials with Electrical resistivity of 6.41E-7 Ω·m | |
600.0 °C | 7.8E-7 Ω·m Show Material materials with Electrical resistivity of 7.8E-7 Ω·m | |
Chemical properties
Property | Value |
---|---|
Carbon | 0.32 - 0.39 % Show Material materials with Carbon of 0.32 - 0.39 % |
Manganese | 0.5 - 0.8 % Show Material materials with Manganese of 0.5 - 0.8 % |
Phosphorus | 0.05 % Show Material materials with Phosphorus of 0.05 % |
Silicon | 0.4 % Show Material materials with Silicon of 0.4 % |
Sulfur | 0.045 % Show Material materials with Sulfur of 0.045 % |
Do you have a technical question or need more information about this material?