DIN 17445 Grade G-X5CrNiMoNb18-10 quenched (+Q)

Want to keep this datasheet? Save it now in your required format

Description

G-X 5 CrNiMoNb 18 10, for armatures pumps, mixers, vessels for the chemical lindustry, cellulose industry, rayon industry, textile industry, rubber industry

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

"Typical" values were obtained via a literature search. "Predicted" values were imputed via artificial intelligence technology. While we have placed significant efforts in ensuring data accuracy, "typical" and "predicted" data should be considered indicative and verified by appropriate material testing. Please do contact us if additional information on the the predicted data method is required.
All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

7.9 g/cm³

Show Material materials with Density of 7.9 g/cm³

Mechanical

PropertyTemperatureValueComment

Elastic modulus

23.0 °C

195 GPa

Show Material materials with Elastic modulus of 195 GPa

Typical for Austenitic Stainless Steel

Elongation

20.0 °C

20 %

Show Material materials with Elongation of 20 %

Hardness, Brinell

20.0 °C

130 - 201 [-]

Show Material materials with Hardness, Brinell of 130 - 201 [-]

Poisson's ratio

23.0 °C

0.3 [-]

Show Material materials with Poisson's ratio of 0.3 [-]

Typical for Austenitic Stainless Steel

Shear modulus

23.0 °C

77 GPa

Show Material materials with Shear modulus of 77 GPa

Typical for Austenitic Stainless Steel

Tensile strength

20.0 °C

440 - 640 MPa

Show Material materials with Tensile strength of 440 - 640 MPa

Yield strength Rp0.2

20.0 °C

185 MPa

Show Material materials with Yield strength Rp0.2 of 185 MPa

100.0 °C

165 - 172 MPa

Show Material materials with Yield strength Rp0.2 of 165 - 172 MPa

150.0 °C

150 - 162 MPa

Show Material materials with Yield strength Rp0.2 of 150 - 162 MPa

200.0 °C

140 - 157 MPa

Show Material materials with Yield strength Rp0.2 of 140 - 157 MPa

250.0 °C

135 - 152 MPa

Show Material materials with Yield strength Rp0.2 of 135 - 152 MPa

300.0 °C

130 - 147 MPa

Show Material materials with Yield strength Rp0.2 of 130 - 147 MPa

350.0 °C

125 - 142 MPa

Show Material materials with Yield strength Rp0.2 of 125 - 142 MPa

400.0 °C

120 - 137 MPa

Show Material materials with Yield strength Rp0.2 of 120 - 137 MPa

450.0 °C

115 - 127 MPa

Show Material materials with Yield strength Rp0.2 of 115 - 127 MPa

500.0 °C

110 - 118 MPa

Show Material materials with Yield strength Rp0.2 of 110 - 118 MPa

550.0 °C

105 - 108 MPa

Show Material materials with Yield strength Rp0.2 of 105 - 108 MPa

Yield strength Rp1.0

20.0 °C

210 MPa

Show Material materials with Yield strength Rp1.0 of 210 MPa

100.0 °C

190 MPa

Show Material materials with Yield strength Rp1.0 of 190 MPa

150.0 °C

175 MPa

Show Material materials with Yield strength Rp1.0 of 175 MPa

200.0 °C

165 MPa

Show Material materials with Yield strength Rp1.0 of 165 MPa

250.0 °C

160 MPa

Show Material materials with Yield strength Rp1.0 of 160 MPa

300.0 °C

155 MPa

Show Material materials with Yield strength Rp1.0 of 155 MPa

350.0 °C

150 MPa

Show Material materials with Yield strength Rp1.0 of 150 MPa

400.0 °C

140 MPa

Show Material materials with Yield strength Rp1.0 of 140 MPa

450.0 °C

130 MPa

Show Material materials with Yield strength Rp1.0 of 130 MPa

500.0 °C

120 MPa

Show Material materials with Yield strength Rp1.0 of 120 MPa

550.0 °C

110 MPa

Show Material materials with Yield strength Rp1.0 of 110 MPa

Unlock all property charts

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

100.0 °C

1.65E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.65E-5 1/K

200.0 °C

1.75E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.75E-5 1/K

300.0 °C

1.8E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.8E-5 1/K

400.0 °C

1.85E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.85E-5 1/K

500.0 °C

1.9E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.9E-5 1/K

Unlock all property charts

Melting point

1230 - 1480 °C

Show Material materials with Melting point of 1230 - 1480 °C

Typical for Austenitic Stainless Steel

Specific heat capacity

20.0 °C

500 J/(kg·K)

Show Material materials with Specific heat capacity of 500 J/(kg·K)

Thermal conductivity

20.0 °C

15 W/(m·K)

Show Material materials with Thermal conductivity of 15 W/(m·K)

Electrical

PropertyTemperatureValue

Electrical conductivity

20.0 °C

1.34E+6 S/m

Show Material materials with Electrical conductivity of 1.34E+6 S/m

Electrical resistivity

20.0 °C

7.7E-7 Ω·m

Show Material materials with Electrical resistivity of 7.7E-7 Ω·m

Chemical properties

PropertyValue

Carbon

0.06 - 0.08 %

Show Material materials with Carbon of 0.06 - 0.08 %

Chromium

17 - 20 %

Show Material materials with Chromium of 17 - 20 %

Manganese

1.5 %

Show Material materials with Manganese of 1.5 %

Molybdenum

2 - 2.5 %

Show Material materials with Molybdenum of 2 - 2.5 %

Nickel

10.5 - 12.5 %

Show Material materials with Nickel of 10.5 - 12.5 %

Phosphorus

0.05 %

Show Material materials with Phosphorus of 0.05 %

Silicon

1.5 %

Show Material materials with Silicon of 1.5 %

Sulfur

0.03 %

Show Material materials with Sulfur of 0.03 %

Technological properties

Property
Processing methods

sand casting and investment casting