General
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Density | 20.0 °C | 2.68 g/cm³ Show Material materials with Density of 2.68 g/cm³ | F22 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 386 |
Mechanical
Property | Temperature | Value | Condition | Related Standards | Comment |
---|---|---|---|---|---|
Elastic modulus | 20.0 °C | 72.0 Show Material materials with Elastic modulus of 72.0 | F22 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 386 | |
Elongation | -196.0 °C | 39.0 % Show Material materials with Elongation of 39.0 % | F22 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 386 | |
-80.0 °C | 30.0 % Show Material materials with Elongation of 30.0 % | F22 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 386 | ||
-28.0 °C | 27.0 % Show Material materials with Elongation of 27.0 % | F22 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 386 | ||
20.0 °C | 25.0 % Show Material materials with Elongation of 25.0 % | F22 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 386 | ||
100.0 °C | 21.0 % Show Material materials with Elongation of 21.0 % | F22 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 386 | ||
150.0 °C | 50.0 % Show Material materials with Elongation of 50.0 % | F22 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 386 | ||
200.0 °C | 60.0 % Show Material materials with Elongation of 60.0 % | F22 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 386 | ||
260.0 °C | 80.0 % Show Material materials with Elongation of 80.0 % | F22 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 386 | ||
315.0 °C | 110.0 % Show Material materials with Elongation of 110.0 % | F22 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 386 | ||
370.0 °C | 130.0 % Show Material materials with Elongation of 130.0 % | F22 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 386 | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | |||
Poisson's ratio | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] | Typical for Wrought 5000 Series Aluminium | |||
Shear modulus | 20.0 °C | 27.0 Show Material materials with Shear modulus of 27.0 | F22 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 386 | |
Tensile strength | -196.0 °C | 370.0 MPa Show Material materials with Tensile strength of 370.0 MPa | F22 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 386 | |
-80.0 °C | 260.0 MPa Show Material materials with Tensile strength of 260.0 MPa | F22 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 386 | ||
-28.0 °C | 250.0 MPa Show Material materials with Tensile strength of 250.0 MPa | F22 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 386 | ||
20.0 °C | 250.0 MPa Show Material materials with Tensile strength of 250.0 MPa | F22 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 386 | ||
100.0 °C | 250.0 MPa Show Material materials with Tensile strength of 250.0 MPa | F22 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 386 | ||
150.0 °C | 200.0 MPa Show Material materials with Tensile strength of 200.0 MPa | F22 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 386 | ||
200.0 °C | 150.0 MPa Show Material materials with Tensile strength of 150.0 MPa | F22 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 386 | ||
260.0 °C | 115.0 MPa Show Material materials with Tensile strength of 115.0 MPa | F22 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 386 | ||
315.0 °C | 75.0 MPa Show Material materials with Tensile strength of 75.0 MPa | F22 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 386 | ||
370.0 °C | 40.0 MPa Show Material materials with Tensile strength of 40.0 MPa | F22 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 386 |
Thermal
Property | Temperature | Value | Condition | Related Standards | Comment |
---|---|---|---|---|---|
Coefficient of thermal expansion | -50.0 °C | 2.19e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.19e-05 1/K | F22 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 386 | |
100.0 °C | 2.37e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.37e-05 1/K | F22 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 386 | ||
200.0 °C | 2.46e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.46e-05 1/K | F22 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 386 | ||
300.0 °C | 2.56e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.56e-05 1/K | F22 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 386 | ||
Max service temperature | 150.0 °C Show Material materials with Max service temperature of 150.0 °C | Typical for Wrought 5000 Series Aluminium | |||
Melting point | 560.0 - 655.0 °C Show Material materials with Melting point of 560.0 - 655.0 °C | Typical for Wrought 5000 Series Aluminium | |||
Specific heat capacity | 20.0 °C | 900.0 J/(kg·K) Show Material materials with Specific heat capacity of 900.0 J/(kg·K) | F22 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 386 | |
Thermal conductivity | 20.0 °C | 150.0 Show Material materials with Thermal conductivity of 150.0 | F22 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 386 |
Electrical
Property | Temperature | Value | Condition | Related Standards | Comment |
---|---|---|---|---|---|
Electrical conductivity | 20.0 °C | 21000000.0 Show Material materials with Electrical conductivity of 21000000.0 | F22 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 386 | |
Electrical resistivity | 3.3e-08 - 5e-08 Ω·m Show Material materials with Electrical resistivity of 3.3e-08 - 5e-08 Ω·m | Typical for Wrought 5000 Series Aluminium |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Chromium | 0.05 - 0.2 % Show Material materials with Chromium of 0.05 - 0.2 % | F22 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 386 |
Copper | 0.1 Show Material materials with Copper of 0.1 | F22 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 386 |
Iron | 0.4 Show Material materials with Iron of 0.4 | F22 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 386 |
Magnesium | 2.4 - 3.0 % Show Material materials with Magnesium of 2.4 - 3.0 % | F22 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 386 |
Manganese | 0.5 - 1.0 % Show Material materials with Manganese of 0.5 - 1.0 % | F22 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 386 |
Silicon | 0.25 Show Material materials with Silicon of 0.25 | F22 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 386 |
Titanium | 0.2 Show Material materials with Titanium of 0.2 | F22 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 386 |
Zinc | 0.25 Show Material materials with Zinc of 0.25 | F22 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 386 |
Technological properties
Property | ||
---|---|---|
Workability | Good workability. |