EN 10025-5 Grade S355J2WP normalized or normalized formed (+N)

Want to keep this datasheet? Save it now in your required format

Description

The weather resistant steel S355J2WP with improved atmospheric corrosion resistance (by generation of an conversion coating) has a minimum yield strength of 355 N/mm². It is applicated for welded, screwed and riveted constructions, e.g. structural engineering, bridge building, tank construction, exhaust systems, vehicle construction, toolbuilding. The grid rate have to considered in the dimensioning process. An conventional surface protection is recommend at polluted air and necessary at long-time water wetting, constant wetness or close to the sea. Unweathered areas with condensate generation have to be adequate ventilated. Before welding the coating have to be removed in a distance of 10 - 20 mm from the welding edge. With increasing thickness, strength and carbon equivalent the occurence of cold cracks in the welding zone is possible. The recommendation of the EURONORM Information No. 2 (EN 1011-2) have to considered. Because of the high amount of P special precautions have to take.

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueComment

Density

23.0 °C

7.9 - 8.2 g/cm³

Show Material materials with Density of 7.9 - 8.2 g/cm³

Typical for Austenitic Stainless Steel

Mechanical

PropertyTemperatureValueComment

Elastic modulus

23.0 °C

195 GPa

Show Material materials with Elastic modulus of 195 GPa

Typical for Austenitic Stainless Steel

Elongation

20.0 °C

22 %

Show Material materials with Elongation of 22 %

Elongation A80

20.0 °C

16 - 18 %

Show Material materials with Elongation A80 of 16 - 18 %

Elongation A80, transverse

20.0 °C

14 - 16 %

Show Material materials with Elongation A80, transverse of 14 - 16 %

Elongation, transverse

20.0 °C

20 %

Show Material materials with Elongation, transverse of 20 %

Poisson's ratio

23.0 °C

0.3 [-]

Show Material materials with Poisson's ratio of 0.3 [-]

Typical for Austenitic Stainless Steel

Shear modulus

23.0 °C

77 GPa

Show Material materials with Shear modulus of 77 GPa

Typical for Austenitic Stainless Steel

Tensile strength

20.0 °C

470 - 680 MPa

Show Material materials with Tensile strength of 470 - 680 MPa

Tensile strength, transverse

20.0 °C

470 - 680 MPa

Show Material materials with Tensile strength, transverse of 470 - 680 MPa

Yield strength

20.0 °C

345 - 355 MPa

Show Material materials with Yield strength of 345 - 355 MPa

Yield strength, transverse

20.0 °C

345 - 355 MPa

Show Material materials with Yield strength, transverse of 345 - 355 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

23.0 °C

1.7E-5 - 1.9E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.7E-5 - 1.9E-5 1/K

Typical for Austenitic Stainless Steel

Melting point

1230 - 1480 °C

Show Material materials with Melting point of 1230 - 1480 °C

Typical for Austenitic Stainless Steel

Specific heat capacity

23.0 °C

440 J/(kg·K)

Show Material materials with Specific heat capacity of 440 J/(kg·K)

Typical for Austenitic Stainless Steel

Thermal conductivity

23.0 °C

11 - 21 W/(m·K)

Show Material materials with Thermal conductivity of 11 - 21 W/(m·K)

Typical for Austenitic Stainless Steel

Electrical

PropertyTemperatureValueComment

Electrical resistivity

23.0 °C

8.5E-7 Ω·m

Show Material materials with Electrical resistivity of 8.5E-7 Ω·m

Typical for Austenitic Stainless Steel

Chemical properties

PropertyValue

Carbon

0.12 %

Show Material materials with Carbon of 0.12 %

Chromium

0.3 - 1.25 %

Show Material materials with Chromium of 0.3 - 1.25 %

Copper

0.25 - 0.55 %

Show Material materials with Copper of 0.25 - 0.55 %

Manganese

1 %

Show Material materials with Manganese of 1 %

Nickel

0.65 %

Show Material materials with Nickel of 0.65 %

Phosphorus

0.06 - 0.15 %

Show Material materials with Phosphorus of 0.06 - 0.15 %

Silicon

0.75 %

Show Material materials with Silicon of 0.75 %

Sulfur

0.03 - 0.035 %

Show Material materials with Sulfur of 0.03 - 0.035 %