EN 10272 Grade X2CrNi19-11 solution annealed (+AT)

Want to keep this datasheet? Save it now in your required format

Description

The austenitic steel grade X2CrNi19-11 acc. to DIN EN 10272 : 2001-01is used for hot and cold formed steels for pressure vessel. It shows resistance to intercrystalline corrosion in delivery condition as well as in sensitized condition due to the lowered c-content.

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

7.9 - 7.92 g/cm³

Show Material materials with Density of 7.9 - 7.92 g/cm³

Mechanical

PropertyTemperatureValue

Elastic modulus

-269.0 °C

201.3 GPa

Show Material materials with Elastic modulus of 201.3 GPa

-195.0 °C

205.1 GPa

Show Material materials with Elastic modulus of 205.1 GPa

-100.0 °C

206 GPa

Show Material materials with Elastic modulus of 206 GPa

20.0 °C

196 - 200 GPa

Show Material materials with Elastic modulus of 196 - 200 GPa

27.0 °C

190.2 GPa

Show Material materials with Elastic modulus of 190.2 GPa

100.0 °C

190 - 194 GPa

Show Material materials with Elastic modulus of 190 - 194 GPa

200.0 °C

182 - 186 GPa

Show Material materials with Elastic modulus of 182 - 186 GPa

300.0 °C

174 - 179 GPa

Show Material materials with Elastic modulus of 174 - 179 GPa

400.0 °C

166 - 172 GPa

Show Material materials with Elastic modulus of 166 - 172 GPa

500.0 °C

158 - 165 GPa

Show Material materials with Elastic modulus of 158 - 165 GPa

600.0 °C

150 GPa

Show Material materials with Elastic modulus of 150 GPa

700.0 °C

142 GPa

Show Material materials with Elastic modulus of 142 GPa

800.0 °C

134 GPa

Show Material materials with Elastic modulus of 134 GPa

Elongation

20.0 °C

45 %

Show Material materials with Elongation of 45 %

Elongation, transverse

20.0 °C

35 %

Show Material materials with Elongation, transverse of 35 %

Hardness, Brinell

20.0 °C

215 [-]

Show Material materials with Hardness, Brinell of 215 [-]

Hardness, Brinell, trans

20.0 °C

215 [-]

Show Material materials with Hardness, Brinell, trans of 215 [-]

Poisson's ratio

-269.0 °C

0.31 [-]

Show Material materials with Poisson's ratio of 0.31 [-]

-195.0 °C

0.29 [-]

Show Material materials with Poisson's ratio of 0.29 [-]

20.0 °C

0.29 [-]

Show Material materials with Poisson's ratio of 0.29 [-]

27.0 °C

0.27 [-]

Show Material materials with Poisson's ratio of 0.27 [-]

Unlock all property charts

Shear modulus

20.0 °C

75.7 GPa

Show Material materials with Shear modulus of 75.7 GPa

Tensile strength

20.0 °C

460 - 680 MPa

Show Material materials with Tensile strength of 460 - 680 MPa

100.0 °C

410 MPa

Show Material materials with Tensile strength of 410 MPa

150.0 °C

380 MPa

Show Material materials with Tensile strength of 380 MPa

200.0 °C

360 MPa

Show Material materials with Tensile strength of 360 MPa

250.0 °C

350 MPa

Show Material materials with Tensile strength of 350 MPa

300.0 °C

340 MPa

Show Material materials with Tensile strength of 340 MPa

350.0 °C

340 MPa

Show Material materials with Tensile strength of 340 MPa

Unlock all property charts

Tensile strength, transverse

20.0 °C

460 - 680 MPa

Show Material materials with Tensile strength, transverse of 460 - 680 MPa

Yield strength Rp0.2

20.0 °C

180 MPa

Show Material materials with Yield strength Rp0.2 of 180 MPa

100.0 °C

145 MPa

Show Material materials with Yield strength Rp0.2 of 145 MPa

150.0 °C

130 MPa

Show Material materials with Yield strength Rp0.2 of 130 MPa

200.0 °C

118 MPa

Show Material materials with Yield strength Rp0.2 of 118 MPa

250.0 °C

108 MPa

Show Material materials with Yield strength Rp0.2 of 108 MPa

300.0 °C

100 MPa

Show Material materials with Yield strength Rp0.2 of 100 MPa

350.0 °C

94 MPa

Show Material materials with Yield strength Rp0.2 of 94 MPa

400.0 °C

89 MPa

Show Material materials with Yield strength Rp0.2 of 89 MPa

450.0 °C

85 MPa

Show Material materials with Yield strength Rp0.2 of 85 MPa

500.0 °C

81 MPa

Show Material materials with Yield strength Rp0.2 of 81 MPa

550.0 °C

80 MPa

Show Material materials with Yield strength Rp0.2 of 80 MPa

Unlock all property charts

Yield strength Rp0.2, transverse

20.0 °C

180 MPa

Show Material materials with Yield strength Rp0.2, transverse of 180 MPa

Yield strength Rp1.0

20.0 °C

215 MPa

Show Material materials with Yield strength Rp1.0 of 215 MPa

100.0 °C

180 MPa

Show Material materials with Yield strength Rp1.0 of 180 MPa

150.0 °C

160 MPa

Show Material materials with Yield strength Rp1.0 of 160 MPa

200.0 °C

145 MPa

Show Material materials with Yield strength Rp1.0 of 145 MPa

250.0 °C

135 MPa

Show Material materials with Yield strength Rp1.0 of 135 MPa

300.0 °C

127 MPa

Show Material materials with Yield strength Rp1.0 of 127 MPa

350.0 °C

121 MPa

Show Material materials with Yield strength Rp1.0 of 121 MPa

400.0 °C

116 MPa

Show Material materials with Yield strength Rp1.0 of 116 MPa

450.0 °C

112 MPa

Show Material materials with Yield strength Rp1.0 of 112 MPa

500.0 °C

109 MPa

Show Material materials with Yield strength Rp1.0 of 109 MPa

550.0 °C

108 MPa

Show Material materials with Yield strength Rp1.0 of 108 MPa

Unlock all property charts

Yield strength Rp1.0, transverse

20.0 °C

215 MPa

Show Material materials with Yield strength Rp1.0, transverse of 215 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

-100.0 °C

1.49E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.49E-5 1/K

20.0 °C

1.61E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.61E-5 1/K

100.0 °C

1.6E-5 - 1.67E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.6E-5 - 1.67E-5 1/K

200.0 °C

1.65E-5 - 1.72E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.65E-5 - 1.72E-5 1/K

300.0 °C

1.7E-5 - 1.77E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.7E-5 - 1.77E-5 1/K

400.0 °C

1.75E-5 - 1.81E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.75E-5 - 1.81E-5 1/K

500.0 °C

1.8E-5 - 1.84E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.8E-5 - 1.84E-5 1/K

600.0 °C

1.88E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.88E-5 1/K

700.0 °C

1.91E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.91E-5 1/K

800.0 °C

1.94E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.94E-5 1/K

Unlock all property charts

Melting point

1230 - 1480 °C

Show Material materials with Melting point of 1230 - 1480 °C

Typical for Austenitic Stainless Steel

Specific heat capacity

-100.0 °C

440 J/(kg·K)

Show Material materials with Specific heat capacity of 440 J/(kg·K)

20.0 °C

472 - 500 J/(kg·K)

Show Material materials with Specific heat capacity of 472 - 500 J/(kg·K)

100.0 °C

487 J/(kg·K)

Show Material materials with Specific heat capacity of 487 J/(kg·K)

200.0 °C

503 J/(kg·K)

Show Material materials with Specific heat capacity of 503 J/(kg·K)

300.0 °C

512 J/(kg·K)

Show Material materials with Specific heat capacity of 512 J/(kg·K)

400.0 °C

520 J/(kg·K)

Show Material materials with Specific heat capacity of 520 J/(kg·K)

500.0 °C

530 J/(kg·K)

Show Material materials with Specific heat capacity of 530 J/(kg·K)

600.0 °C

541 J/(kg·K)

Show Material materials with Specific heat capacity of 541 J/(kg·K)

700.0 °C

551 J/(kg·K)

Show Material materials with Specific heat capacity of 551 J/(kg·K)

800.0 °C

559 J/(kg·K)

Show Material materials with Specific heat capacity of 559 J/(kg·K)

Unlock all property charts

Thermal conductivity

20.0 °C

13.9 - 15 W/(m·K)

Show Material materials with Thermal conductivity of 13.9 - 15 W/(m·K)

100.0 °C

15.4 W/(m·K)

Show Material materials with Thermal conductivity of 15.4 W/(m·K)

200.0 °C

17.2 W/(m·K)

Show Material materials with Thermal conductivity of 17.2 W/(m·K)

300.0 °C

18.7 W/(m·K)

Show Material materials with Thermal conductivity of 18.7 W/(m·K)

400.0 °C

20.2 W/(m·K)

Show Material materials with Thermal conductivity of 20.2 W/(m·K)

500.0 °C

21.6 W/(m·K)

Show Material materials with Thermal conductivity of 21.6 W/(m·K)

600.0 °C

23 W/(m·K)

Show Material materials with Thermal conductivity of 23 W/(m·K)

700.0 °C

24.4 W/(m·K)

Show Material materials with Thermal conductivity of 24.4 W/(m·K)

800.0 °C

25.8 W/(m·K)

Show Material materials with Thermal conductivity of 25.8 W/(m·K)

Unlock all property charts

Thermal diffusivity

20.0 °C

3.7 mm²/s

Show Material materials with Thermal diffusivity of 3.7 mm²/s

100.0 °C

3.9 mm²/s

Show Material materials with Thermal diffusivity of 3.9 mm²/s

200.0 °C

4.2 mm²/s

Show Material materials with Thermal diffusivity of 4.2 mm²/s

300.0 °C

4.5 mm²/s

Show Material materials with Thermal diffusivity of 4.5 mm²/s

400.0 °C

4.7 mm²/s

Show Material materials with Thermal diffusivity of 4.7 mm²/s

500.0 °C

4.8 mm²/s

Show Material materials with Thermal diffusivity of 4.8 mm²/s

600.0 °C

5 mm²/s

Show Material materials with Thermal diffusivity of 5 mm²/s

700.0 °C

5.3 mm²/s

Show Material materials with Thermal diffusivity of 5.3 mm²/s

800.0 °C

5.6 mm²/s

Show Material materials with Thermal diffusivity of 5.6 mm²/s

Unlock all property charts

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

7.3E-7 - 7.35E-7 Ω·m

Show Material materials with Electrical resistivity of 7.3E-7 - 7.35E-7 Ω·m

100.0 °C

8E-7 Ω·m

Show Material materials with Electrical resistivity of 8E-7 Ω·m

200.0 °C

8.68E-7 Ω·m

Show Material materials with Electrical resistivity of 8.68E-7 Ω·m

300.0 °C

9.33E-7 Ω·m

Show Material materials with Electrical resistivity of 9.33E-7 Ω·m

400.0 °C

9.89E-7 Ω·m

Show Material materials with Electrical resistivity of 9.89E-7 Ω·m

500.0 °C

1.04E-6 Ω·m

Show Material materials with Electrical resistivity of 1.04E-6 Ω·m

600.0 °C

1.08E-6 Ω·m

Show Material materials with Electrical resistivity of 1.08E-6 Ω·m

700.0 °C

1.12E-6 Ω·m

Show Material materials with Electrical resistivity of 1.12E-6 Ω·m

800.0 °C

1.15E-6 Ω·m

Show Material materials with Electrical resistivity of 1.15E-6 Ω·m

Unlock all property charts

Chemical properties

PropertyValue

Carbon

0.03 %

Show Material materials with Carbon of 0.03 %

Chromium

18 - 20 %

Show Material materials with Chromium of 18 - 20 %

Manganese

2 %

Show Material materials with Manganese of 2 %

Nickel

10 - 12 %

Show Material materials with Nickel of 10 - 12 %

Nitrogen

0.1 - 0.11 %

Show Material materials with Nitrogen of 0.1 - 0.11 %

Phosphorus

0.05 %

Show Material materials with Phosphorus of 0.05 %

Silicon

1 %

Show Material materials with Silicon of 1 %

Sulfur

0.015 - 0.03 %

Show Material materials with Sulfur of 0.015 - 0.03 %