EN 10272 Grade X12Cr13 soft annealed (+A)

Want to keep this datasheet? Save it now in your required format

Description

The martensitic steel grade X12Cr13 acc. to DIN EN 10272 : 2001-01 is used for hot and cold formed rods for pressure vessels.

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

7.73 g/cm³

Show Material materials with Density of 7.73 g/cm³

Mechanical

PropertyTemperatureValue

Elastic modulus

20.0 °C

217 - 217.99 GPa

Show Material materials with Elastic modulus of 217 - 217.99 GPa

100.0 °C

213.2 - 215 GPa

Show Material materials with Elastic modulus of 213.2 - 215 GPa

200.0 °C

188 - 205.94 GPa

Show Material materials with Elastic modulus of 188 - 205.94 GPa

300.0 °C

164 - 198.53 GPa

Show Material materials with Elastic modulus of 164 - 198.53 GPa

400.0 °C

188.79 GPa

Show Material materials with Elastic modulus of 188.79 GPa

Hardness, Brinell

20.0 °C

220 [-]

Show Material materials with Hardness, Brinell of 220 [-]

Poisson's ratio

20.0 °C

0.29 [-]

Show Material materials with Poisson's ratio of 0.29 [-]

100.0 °C

0.29 [-]

Show Material materials with Poisson's ratio of 0.29 [-]

200.0 °C

0.29 [-]

Show Material materials with Poisson's ratio of 0.29 [-]

300.0 °C

0.31 [-]

Show Material materials with Poisson's ratio of 0.31 [-]

400.0 °C

0.31 [-]

Show Material materials with Poisson's ratio of 0.31 [-]

Unlock all property charts

Shear modulus

20.0 °C

84.82 GPa

Show Material materials with Shear modulus of 84.82 GPa

100.0 °C

82.5 GPa

Show Material materials with Shear modulus of 82.5 GPa

200.0 °C

79.57 GPa

Show Material materials with Shear modulus of 79.57 GPa

300.0 °C

75.86 GPa

Show Material materials with Shear modulus of 75.86 GPa

400.0 °C

72 GPa

Show Material materials with Shear modulus of 72 GPa

Unlock all property charts

Tensile strength

20.0 °C

730 MPa

Show Material materials with Tensile strength of 730 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

20.0 °C

1.02E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.02E-5 1/K

100.0 °C

1.05E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.05E-5 1/K

200.0 °C

1.09E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.09E-5 1/K

300.0 °C

1.13E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.13E-5 1/K

400.0 °C

1.16E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.16E-5 1/K

500.0 °C

1.2E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.2E-5 1/K

600.0 °C

1.22E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.22E-5 1/K

Unlock all property charts

Melting point

1370 - 1530 °C

Show Material materials with Melting point of 1370 - 1530 °C

Typical for Martensitic Stainless Steel

Specific heat capacity

20.0 °C

439 J/(kg·K)

Show Material materials with Specific heat capacity of 439 J/(kg·K)

100.0 °C

474 J/(kg·K)

Show Material materials with Specific heat capacity of 474 J/(kg·K)

200.0 °C

498 J/(kg·K)

Show Material materials with Specific heat capacity of 498 J/(kg·K)

300.0 °C

517 J/(kg·K)

Show Material materials with Specific heat capacity of 517 J/(kg·K)

400.0 °C

538 J/(kg·K)

Show Material materials with Specific heat capacity of 538 J/(kg·K)

500.0 °C

564 J/(kg·K)

Show Material materials with Specific heat capacity of 564 J/(kg·K)

600.0 °C

598 J/(kg·K)

Show Material materials with Specific heat capacity of 598 J/(kg·K)

Unlock all property charts

Thermal conductivity

20.0 °C

25.9 W/(m·K)

Show Material materials with Thermal conductivity of 25.9 W/(m·K)

100.0 °C

25.3 W/(m·K)

Show Material materials with Thermal conductivity of 25.3 W/(m·K)

200.0 °C

25.2 W/(m·K)

Show Material materials with Thermal conductivity of 25.2 W/(m·K)

300.0 °C

25.2 W/(m·K)

Show Material materials with Thermal conductivity of 25.2 W/(m·K)

400.0 °C

25.4 W/(m·K)

Show Material materials with Thermal conductivity of 25.4 W/(m·K)

500.0 °C

25.7 W/(m·K)

Show Material materials with Thermal conductivity of 25.7 W/(m·K)

600.0 °C

25.9 W/(m·K)

Show Material materials with Thermal conductivity of 25.9 W/(m·K)

Unlock all property charts

Thermal diffusivity

20.0 °C

7.6 mm²/s

Show Material materials with Thermal diffusivity of 7.6 mm²/s

100.0 °C

6.6 mm²/s

Show Material materials with Thermal diffusivity of 6.6 mm²/s

200.0 °C

6.1 mm²/s

Show Material materials with Thermal diffusivity of 6.1 mm²/s

300.0 °C

5.8 mm²/s

Show Material materials with Thermal diffusivity of 5.8 mm²/s

400.0 °C

5.3 mm²/s

Show Material materials with Thermal diffusivity of 5.3 mm²/s

500.0 °C

4.8 mm²/s

Show Material materials with Thermal diffusivity of 4.8 mm²/s

600.0 °C

4.1 mm²/s

Show Material materials with Thermal diffusivity of 4.1 mm²/s

Unlock all property charts

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

5.59E-7 Ω·m

Show Material materials with Electrical resistivity of 5.59E-7 Ω·m

100.0 °C

6.4E-7 Ω·m

Show Material materials with Electrical resistivity of 6.4E-7 Ω·m

200.0 °C

7.32E-7 Ω·m

Show Material materials with Electrical resistivity of 7.32E-7 Ω·m

300.0 °C

8.17E-7 Ω·m

Show Material materials with Electrical resistivity of 8.17E-7 Ω·m

400.0 °C

8.97E-7 Ω·m

Show Material materials with Electrical resistivity of 8.97E-7 Ω·m

500.0 °C

9.74E-7 Ω·m

Show Material materials with Electrical resistivity of 9.74E-7 Ω·m

600.0 °C

1.05E-6 Ω·m

Show Material materials with Electrical resistivity of 1.05E-6 Ω·m

Unlock all property charts

Chemical properties

PropertyValue

Carbon

0.08 - 0.15 %

Show Material materials with Carbon of 0.08 - 0.15 %

Chromium

11.5 - 13.5 %

Show Material materials with Chromium of 11.5 - 13.5 %

Manganese

1.5 %

Show Material materials with Manganese of 1.5 %

Nickel

0.75 %

Show Material materials with Nickel of 0.75 %

Phosphorus

0.04 %

Show Material materials with Phosphorus of 0.04 %

Silicon

1 %

Show Material materials with Silicon of 1 %

Sulfur

0.015 - 0.03 %

Show Material materials with Sulfur of 0.015 - 0.03 %