EN 10269 Grade X10CrNiMoMnNbVB15-10-1 solution heat-treated and warm worked (+AT+WW)

Want to keep this datasheet? Save it now in your required format

Description

Application for mounting elements at increased temperatures.

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

7.95 g/cm³

Show Material materials with Density of 7.95 g/cm³

Mechanical

PropertyTemperatureValueComment

Elastic modulus

20.0 °C

207 GPa

Show Material materials with Elastic modulus of 207 GPa

100.0 °C

201 GPa

Show Material materials with Elastic modulus of 201 GPa

200.0 °C

193 GPa

Show Material materials with Elastic modulus of 193 GPa

300.0 °C

184 GPa

Show Material materials with Elastic modulus of 184 GPa

400.0 °C

175 GPa

Show Material materials with Elastic modulus of 175 GPa

500.0 °C

165 GPa

Show Material materials with Elastic modulus of 165 GPa

600.0 °C

158 GPa

Show Material materials with Elastic modulus of 158 GPa

700.0 °C

150 GPa

Show Material materials with Elastic modulus of 150 GPa

Elongation

20.0 °C

25 %

Show Material materials with Elongation of 25 %

Poisson's ratio

23.0 °C

0.3 [-]

Show Material materials with Poisson's ratio of 0.3 [-]

Typical for Austenitic Stainless Steel

Shear modulus

23.0 °C

77 GPa

Show Material materials with Shear modulus of 77 GPa

Typical for Austenitic Stainless Steel

Tensile strength

20.0 °C

650 - 850 MPa

Show Material materials with Tensile strength of 650 - 850 MPa

50.0 °C

610 MPa

Show Material materials with Tensile strength of 610 MPa

100.0 °C

565 MPa

Show Material materials with Tensile strength of 565 MPa

150.0 °C

530 MPa

Show Material materials with Tensile strength of 530 MPa

200.0 °C

505 MPa

Show Material materials with Tensile strength of 505 MPa

250.0 °C

490 MPa

Show Material materials with Tensile strength of 490 MPa

300.0 °C

475 MPa

Show Material materials with Tensile strength of 475 MPa

350.0 °C

465 MPa

Show Material materials with Tensile strength of 465 MPa

400.0 °C

460 MPa

Show Material materials with Tensile strength of 460 MPa

450.0 °C

450 MPa

Show Material materials with Tensile strength of 450 MPa

500.0 °C

440 MPa

Show Material materials with Tensile strength of 440 MPa

550.0 °C

430 MPa

Show Material materials with Tensile strength of 430 MPa

600.0 °C

410 MPa

Show Material materials with Tensile strength of 410 MPa

650.0 °C

390 MPa

Show Material materials with Tensile strength of 390 MPa

Unlock all property charts

Yield strength Rp0.2

20.0 °C

510 MPa

Show Material materials with Yield strength Rp0.2 of 510 MPa

50.0 °C

490 MPa

Show Material materials with Yield strength Rp0.2 of 490 MPa

100.0 °C

463 MPa

Show Material materials with Yield strength Rp0.2 of 463 MPa

150.0 °C

446 MPa

Show Material materials with Yield strength Rp0.2 of 446 MPa

200.0 °C

434 MPa

Show Material materials with Yield strength Rp0.2 of 434 MPa

250.0 °C

423 MPa

Show Material materials with Yield strength Rp0.2 of 423 MPa

300.0 °C

413 MPa

Show Material materials with Yield strength Rp0.2 of 413 MPa

350.0 °C

405 MPa

Show Material materials with Yield strength Rp0.2 of 405 MPa

400.0 °C

396 MPa

Show Material materials with Yield strength Rp0.2 of 396 MPa

450.0 °C

391 MPa

Show Material materials with Yield strength Rp0.2 of 391 MPa

500.0 °C

386 MPa

Show Material materials with Yield strength Rp0.2 of 386 MPa

550.0 °C

378 MPa

Show Material materials with Yield strength Rp0.2 of 378 MPa

600.0 °C

365 MPa

Show Material materials with Yield strength Rp0.2 of 365 MPa

650.0 °C

346 MPa

Show Material materials with Yield strength Rp0.2 of 346 MPa

Unlock all property charts

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

100.0 °C

1.57E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.57E-5 1/K

200.0 °C

1.68E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.68E-5 1/K

300.0 °C

1.77E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.77E-5 1/K

400.0 °C

1.83E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.83E-5 1/K

500.0 °C

1.86E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.86E-5 1/K

600.0 °C

1.9E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.9E-5 1/K

Unlock all property charts

Melting point

1230 - 1480 °C

Show Material materials with Melting point of 1230 - 1480 °C

Typical for Austenitic Stainless Steel

Specific heat capacity

20.0 °C

480 J/(kg·K)

Show Material materials with Specific heat capacity of 480 J/(kg·K)

Thermal conductivity

20.0 °C

12.5 W/(m·K)

Show Material materials with Thermal conductivity of 12.5 W/(m·K)

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

7.4E-7 Ω·m

Show Material materials with Electrical resistivity of 7.4E-7 Ω·m

Chemical properties

PropertyValue

Boron

3E-3 - 9E-3 %

Show Material materials with Boron of 3E-3 - 9E-3 %

Carbon

0.07 - 0.13 %

Show Material materials with Carbon of 0.07 - 0.13 %

Chromium

14 - 16 %

Show Material materials with Chromium of 14 - 16 %

Manganese

5.5 - 7 %

Show Material materials with Manganese of 5.5 - 7 %

Molybdenum

0.8 - 1.2 %

Show Material materials with Molybdenum of 0.8 - 1.2 %

Nickel

9 - 11 %

Show Material materials with Nickel of 9 - 11 %

Niobium

0.75 - 1.25 %

Show Material materials with Niobium of 0.75 - 1.25 %

Nitrogen

0.1 - 0.11 %

Show Material materials with Nitrogen of 0.1 - 0.11 %

Phosphorus

0.04 %

Show Material materials with Phosphorus of 0.04 %

Silicon

1 %

Show Material materials with Silicon of 1 %

Sulfur

0.015 - 0.03 %

Show Material materials with Sulfur of 0.015 - 0.03 %

Vanadium

0.15 - 0.4 %

Show Material materials with Vanadium of 0.15 - 0.4 %