General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Density | 20 °C | 7.8 g/cm³ Show Material materials with Density of 7.8 g/cm³ | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat |
20 °C | 7.8 - 7.85 g/cm³ Show Material materials with Density of 7.8 - 7.85 g/cm³ | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | |
20 °C | 7.85 g/cm³ Show Material materials with Density of 7.85 g/cm³ | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat |
Mechanical
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Elastic modulus | -100 °C | 217 GPa Show Material materials with Elastic modulus of 217 GPa | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | |
20 °C | 210 - 212 GPa Show Material materials with Elastic modulus of 210 - 212 GPa | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
20 °C | 210 GPa Show Material materials with Elastic modulus of 210 GPa | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
20 °C | 212 GPa Show Material materials with Elastic modulus of 212 GPa | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
100 °C | 205 - 207 GPa Show Material materials with Elastic modulus of 205 - 207 GPa | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
100 °C | 205 GPa Show Material materials with Elastic modulus of 205 GPa | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
100 °C | 207 GPa Show Material materials with Elastic modulus of 207 GPa | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
200 °C | 195 - 199 GPa Show Material materials with Elastic modulus of 195 - 199 GPa | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
200 °C | 195 GPa Show Material materials with Elastic modulus of 195 GPa | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
200 °C | 199 GPa Show Material materials with Elastic modulus of 199 GPa | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
300 °C | 185 - 192 GPa Show Material materials with Elastic modulus of 185 - 192 GPa | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
300 °C | 185 GPa Show Material materials with Elastic modulus of 185 GPa | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
300 °C | 192 GPa Show Material materials with Elastic modulus of 192 GPa | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
400 °C | 175 - 184 GPa Show Material materials with Elastic modulus of 175 - 184 GPa | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
400 °C | 175 GPa Show Material materials with Elastic modulus of 175 GPa | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
400 °C | 184 GPa Show Material materials with Elastic modulus of 184 GPa | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
500 °C | 175 GPa Show Material materials with Elastic modulus of 175 GPa | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
600 °C | 164 GPa Show Material materials with Elastic modulus of 164 GPa | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
Elongation | 12.1 % Show Material materials with Elongation of 12.1 % | Predicted Value, A200 | ||||
12.5 % Show Material materials with Elongation of 12.5 % | Predicted Value, A80 | |||||
17.3 % Show Material materials with Elongation of 17.3 % | Predicted Value, A50 | |||||
18.1 % Show Material materials with Elongation of 18.1 % | Predicted Value, A80 Transverse | |||||
18.4 % Show Material materials with Elongation of 18.4 % | Predicted Value, A5 | |||||
20 °C | 11 % Show Material materials with Elongation of 11 % | quenched and tempered (+QT) | EN 10083-2, ISO 683-1 | Forging | Transverse | |
20 °C | 12 % Show Material materials with Elongation of 12 % | quenched and tempered (+QT) | EN 10083-2, ISO 683-1 | Forging | Transverse | |
20 °C | 14 % Show Material materials with Elongation of 14 % | quenched and tempered (+QT) | ISO 683-1, EN 10083-2, EN 10083-1, EN 10083-3 | Bar, Forging, Sheet, Strip, Flat | ||
20 °C | 16 % Show Material materials with Elongation of 16 % | quenched and tempered (+QT) | ISO 683-1, EN 10083-2, EN 10083-1, EN 10083-3 | Bar, Forging, Sheet, Strip, Flat | ||
20 °C | 17 % Show Material materials with Elongation of 17 % | quenched and tempered (+QT) | ISO 683-1, EN 10083-2, EN 10083-1, EN 10083-3 | Bar, Forging, Sheet, Strip, Flat | ||
20 °C | 18 % Show Material materials with Elongation of 18 % | quenched and tempered (+QT) | EN 10083-2, ISO 683-1 | Forging | ||
Poisson's ratio | 0.29 [-] Show Material materials with Poisson's ratio of 0.29 [-] | Typical for Medium Carbon Steel | ||||
Reduction of area | 40.8 % Show Material materials with Reduction of area of 40.8 % | Predicted Value, Transverse | ||||
20 °C | 35 % Show Material materials with Reduction of area of 35 % | quenched and tempered (+QT) | ISO 683-1, EN 10083-2, EN 10083-1, EN 10083-3 | Bar, Forging, Sheet, Strip, Flat | ||
20 °C | 40 % Show Material materials with Reduction of area of 40 % | quenched and tempered (+QT) | ISO 683-1, EN 10083-2, EN 10083-1, EN 10083-3 | Bar, Forging, Sheet, Strip, Flat | ||
20 °C | 45 % Show Material materials with Reduction of area of 45 % | quenched and tempered (+QT) | ISO 683-1, EN 10083-2, EN 10083-1, EN 10083-3 | Bar, Forging, Sheet, Strip, Flat | ||
Shear modulus | 20 °C | 81 GPa Show Material materials with Shear modulus of 81 GPa | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | |
Shear strength | 516.2 MPa Show Material materials with Shear strength of 516.2 MPa | Predicted Value | ||||
Tensile strength | 20 °C | 590 - 740 MPa Show Material materials with Tensile strength of 590 - 740 MPa | quenched and tempered (+QT) | EN 10083-2, ISO 683-1 | Forging | |
20 °C | 630 - 850 MPa Show Material materials with Tensile strength of 630 - 850 MPa | quenched and tempered (+QT) | ISO 683-1, EN 10083-2, EN 10083-1, EN 10083-3 | Bar, Forging, Sheet, Strip, Flat | ||
20 °C | 630 - 800 MPa Show Material materials with Tensile strength of 630 - 800 MPa | quenched and tempered (+QT) | ISO 683-1, EN 10083-2, EN 10083-1, EN 10083-3 | Bar, Forging, Sheet, Strip, Flat | ||
20 °C | 630 - 780 MPa Show Material materials with Tensile strength of 630 - 780 MPa | quenched and tempered (+QT) | ISO 683-1, EN 10083-2, EN 10083-1, EN 10083-3 | Bar, Forging, Sheet, Strip, Flat | ||
20 °C | 650 - 850 MPa Show Material materials with Tensile strength of 650 - 850 MPa | quenched and tempered (+QT) | ISO 683-1, EN 10083-2, EN 10083-1, EN 10083-3 | Bar, Forging, Sheet, Strip, Flat | ||
20 °C | 650 - 800 MPa Show Material materials with Tensile strength of 650 - 800 MPa | quenched and tempered (+QT) | ISO 683-1, EN 10083-2, EN 10083-1, EN 10083-3 | Bar, Forging, Sheet, Strip, Flat | ||
20 °C | 650 - 780 MPa Show Material materials with Tensile strength of 650 - 780 MPa | quenched and tempered (+QT) | ISO 683-1, EN 10083-2, EN 10083-1, EN 10083-3 | Bar, Forging, Sheet, Strip, Flat | ||
20 °C | 700 - 850 MPa Show Material materials with Tensile strength of 700 - 850 MPa | quenched and tempered (+QT) | ISO 683-1, EN 10083-2, EN 10083-1, EN 10083-3 | Bar, Forging, Sheet, Strip, Flat | ||
20 °C | 700 - 800 MPa Show Material materials with Tensile strength of 700 - 800 MPa | quenched and tempered (+QT) | ISO 683-1, EN 10083-2, EN 10083-1, EN 10083-3 | Bar, Forging, Sheet, Strip, Flat | ||
20 °C | 700 - 780 MPa Show Material materials with Tensile strength of 700 - 780 MPa | quenched and tempered (+QT) | ISO 683-1, EN 10083-2, EN 10083-1, EN 10083-3 | Bar, Forging, Sheet, Strip, Flat | ||
Yield strength | 283.1 MPa Show Material materials with Yield strength of 283.1 MPa | Predicted Value, RP1 | ||||
319 MPa Show Material materials with Yield strength of 319 MPa | Predicted Value, RP05 | |||||
324.8 MPa Show Material materials with Yield strength of 324.8 MPa | Predicted Value, RP1 Transverse | |||||
373.1 MPa Show Material materials with Yield strength of 373.1 MPa | Predicted Value, Transverse | |||||
474 MPa Show Material materials with Yield strength of 474 MPa | Predicted Value, RP02 Transverse | |||||
502.9 MPa Show Material materials with Yield strength of 502.9 MPa | Predicted Value, RP02 | |||||
539.5 MPa Show Material materials with Yield strength of 539.5 MPa | Predicted Value, RP002 | |||||
20 °C | 325 MPa Show Material materials with Yield strength of 325 MPa | quenched and tempered (+QT) | EN 10083-2, ISO 683-1 | Forging | ||
20 °C | 345 MPa Show Material materials with Yield strength of 345 MPa | quenched and tempered (+QT) | EN 10083-2, ISO 683-1 | Forging | ||
20 °C | 370 MPa Show Material materials with Yield strength of 370 MPa | quenched and tempered (+QT) | ISO 683-1, EN 10083-2, EN 10083-1, EN 10083-3 | Bar, Forging, Sheet, Strip, Flat | ||
20 °C | 430 MPa Show Material materials with Yield strength of 430 MPa | quenched and tempered (+QT) | ISO 683-1, EN 10083-2, EN 10083-1, EN 10083-3 | Bar, Forging, Sheet, Strip, Flat | ||
20 °C | 490 MPa Show Material materials with Yield strength of 490 MPa | quenched and tempered (+QT) | ISO 683-1, EN 10083-2, EN 10083-1, EN 10083-3 | Bar, Forging, Sheet, Strip, Flat | ||
100 °C | 294 MPa Show Material materials with Yield strength of 294 MPa | quenched and tempered (+QT) | EN 10083-2, ISO 683-1 | Forging | ||
100 °C | 314 MPa Show Material materials with Yield strength of 314 MPa | quenched and tempered (+QT) | EN 10083-2, ISO 683-1 | Forging | ||
200 °C | 265 MPa Show Material materials with Yield strength of 265 MPa | quenched and tempered (+QT) | EN 10083-2, ISO 683-1 | Forging | ||
200 °C | 284 MPa Show Material materials with Yield strength of 284 MPa | quenched and tempered (+QT) | EN 10083-2, ISO 683-1 | Forging | ||
250 °C | 245 MPa Show Material materials with Yield strength of 245 MPa | quenched and tempered (+QT) | EN 10083-2, ISO 683-1 | Forging | ||
250 °C | 255 MPa Show Material materials with Yield strength of 255 MPa | quenched and tempered (+QT) | EN 10083-2, ISO 683-1 | Forging | ||
300 °C | 226 MPa Show Material materials with Yield strength of 226 MPa | quenched and tempered (+QT) | EN 10083-2, ISO 683-1 | Forging | ||
300 °C | 235 MPa Show Material materials with Yield strength of 235 MPa | quenched and tempered (+QT) | EN 10083-2, ISO 683-1 | Forging | ||
350 °C | 196 MPa Show Material materials with Yield strength of 196 MPa | quenched and tempered (+QT) | EN 10083-2, ISO 683-1 | Forging | ||
350 °C | 206 MPa Show Material materials with Yield strength of 206 MPa | quenched and tempered (+QT) | EN 10083-2, ISO 683-1 | Forging |
Thermal
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coefficient of thermal expansion | -100 °C | 1.08e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.08e-05 1/K | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | |
20 °C | 1.19e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.19e-05 1/K | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
100 °C | 1.11e-05 - 1.25e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.11e-05 - 1.25e-05 1/K | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
100 °C | 1.11e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.11e-05 1/K | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
100 °C | 1.25e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.25e-05 1/K | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
200 °C | 1.21e-05 - 1.3e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.21e-05 - 1.3e-05 1/K | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
200 °C | 1.21e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.21e-05 1/K | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
200 °C | 1.3e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.3e-05 1/K | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
300 °C | 1.29e-05 - 1.36e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.29e-05 - 1.36e-05 1/K | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
300 °C | 1.29e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.29e-05 1/K | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
300 °C | 1.36e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.36e-05 1/K | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
400 °C | 1.35e-05 - 1.41e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.35e-05 - 1.41e-05 1/K | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
400 °C | 1.35e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.35e-05 1/K | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
400 °C | 1.41e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.41e-05 1/K | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
500 °C | 1.45e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.45e-05 1/K | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
600 °C | 1.49e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.49e-05 1/K | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
Max service temperature | -25 - 480 °C Show Material materials with Max service temperature of -25 - 480 °C | quenched and tempered (+QT) | EN 10083-1, EN 10083-2, EN 10083-3 | Bar, Forging, Sheet, Strip, Flat | Long | |
500 °C Show Material materials with Max service temperature of 500 °C | Typical for Carbon Steel | |||||
Melting point | 1380 - 1514 °C Show Material materials with Melting point of 1380 - 1514 °C | Typical for Medium Carbon Steel | ||||
Specific heat capacity | -100 °C | 423 J/(kg·K) Show Material materials with Specific heat capacity of 423 J/(kg·K) | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | |
20 °C | 461 J/(kg·K) Show Material materials with Specific heat capacity of 461 J/(kg·K) | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
20 °C | 461 - 480 J/(kg·K) Show Material materials with Specific heat capacity of 461 - 480 J/(kg·K) | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
20 °C | 480 J/(kg·K) Show Material materials with Specific heat capacity of 480 J/(kg·K) | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
100 °C | 479 J/(kg·K) Show Material materials with Specific heat capacity of 479 J/(kg·K) | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
100 °C | 479 - 500 J/(kg·K) Show Material materials with Specific heat capacity of 479 - 500 J/(kg·K) | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
100 °C | 500 J/(kg·K) Show Material materials with Specific heat capacity of 500 J/(kg·K) | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
200 °C | 499 J/(kg·K) Show Material materials with Specific heat capacity of 499 J/(kg·K) | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
200 °C | 499 - 550 J/(kg·K) Show Material materials with Specific heat capacity of 499 - 550 J/(kg·K) | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
200 °C | 550 J/(kg·K) Show Material materials with Specific heat capacity of 550 J/(kg·K) | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
300 °C | 517 J/(kg·K) Show Material materials with Specific heat capacity of 517 J/(kg·K) | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
300 °C | 517 - 590 J/(kg·K) Show Material materials with Specific heat capacity of 517 - 590 J/(kg·K) | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
300 °C | 590 J/(kg·K) Show Material materials with Specific heat capacity of 590 J/(kg·K) | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
400 °C | 536 J/(kg·K) Show Material materials with Specific heat capacity of 536 J/(kg·K) | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
500 °C | 558 J/(kg·K) Show Material materials with Specific heat capacity of 558 J/(kg·K) | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
600 °C | 587 J/(kg·K) Show Material materials with Specific heat capacity of 587 J/(kg·K) | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
Thermal conductivity | 20 °C | 41.7 W/(m·K) Show Material materials with Thermal conductivity of 41.7 W/(m·K) | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | |
20 °C | 41.7 - 52 W/(m·K) Show Material materials with Thermal conductivity of 41.7 - 52 W/(m·K) | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
20 °C | 52 W/(m·K) Show Material materials with Thermal conductivity of 52 W/(m·K) | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
100 °C | 43.4 W/(m·K) Show Material materials with Thermal conductivity of 43.4 W/(m·K) | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
100 °C | 43.4 - 50.6 W/(m·K) Show Material materials with Thermal conductivity of 43.4 - 50.6 W/(m·K) | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
100 °C | 50.6 W/(m·K) Show Material materials with Thermal conductivity of 50.6 W/(m·K) | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
200 °C | 43.2 W/(m·K) Show Material materials with Thermal conductivity of 43.2 W/(m·K) | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
200 °C | 43.2 - 48.1 W/(m·K) Show Material materials with Thermal conductivity of 43.2 - 48.1 W/(m·K) | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
200 °C | 48.1 W/(m·K) Show Material materials with Thermal conductivity of 48.1 W/(m·K) | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
300 °C | 41.4 W/(m·K) Show Material materials with Thermal conductivity of 41.4 W/(m·K) | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
300 °C | 41.4 - 45.7 W/(m·K) Show Material materials with Thermal conductivity of 41.4 - 45.7 W/(m·K) | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
300 °C | 45.7 W/(m·K) Show Material materials with Thermal conductivity of 45.7 W/(m·K) | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
400 °C | 39.1 W/(m·K) Show Material materials with Thermal conductivity of 39.1 W/(m·K) | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
500 °C | 36.7 W/(m·K) Show Material materials with Thermal conductivity of 36.7 W/(m·K) | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
600 °C | 34.1 W/(m·K) Show Material materials with Thermal conductivity of 34.1 W/(m·K) | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
Thermal diffusivity | 20 °C | 11.6 mm²/s Show Material materials with Thermal diffusivity of 11.6 mm²/s | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | |
100 °C | 11.3 mm²/s Show Material materials with Thermal diffusivity of 11.3 mm²/s | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
200 °C | 10.5 mm²/s Show Material materials with Thermal diffusivity of 10.5 mm²/s | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
300 °C | 9.5 mm²/s Show Material materials with Thermal diffusivity of 9.5 mm²/s | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
400 °C | 8.3 mm²/s Show Material materials with Thermal diffusivity of 8.3 mm²/s | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
500 °C | 7.1 mm²/s Show Material materials with Thermal diffusivity of 7.1 mm²/s | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
600 °C | 5.8 mm²/s Show Material materials with Thermal diffusivity of 5.8 mm²/s | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat |
Electrical
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Electrical conductivity | 5 S/m Show Material materials with Electrical conductivity of 5 S/m | Predicted Value | ||||
Electrical resistivity | 20 °C | 1.2e-07 - 2.5e-07 Ω·m Show Material materials with Electrical resistivity of 1.2e-07 - 2.5e-07 Ω·m | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | |
20 °C | 1.2e-07 Ω·m Show Material materials with Electrical resistivity of 1.2e-07 Ω·m | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
20 °C | 2.5e-07 Ω·m Show Material materials with Electrical resistivity of 2.5e-07 Ω·m | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
100 °C | 2.95e-07 Ω·m Show Material materials with Electrical resistivity of 2.95e-07 Ω·m | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
200 °C | 3.65e-07 Ω·m Show Material materials with Electrical resistivity of 3.65e-07 Ω·m | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
300 °C | 4.53e-07 Ω·m Show Material materials with Electrical resistivity of 4.53e-07 Ω·m | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
400 °C | 5.56e-07 Ω·m Show Material materials with Electrical resistivity of 5.56e-07 Ω·m | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
500 °C | 6.74e-07 Ω·m Show Material materials with Electrical resistivity of 6.74e-07 Ω·m | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat | ||
600 °C | 8.13e-07 Ω·m Show Material materials with Electrical resistivity of 8.13e-07 Ω·m | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Carbon | 0.42 - 0.5 % Show Material materials with Carbon of 0.42 - 0.5 % | quenched and tempered (+QT) | ISO 683-1, EN 10083-2, EN 10083-1, EN 10083-3 | Bar, Forging, Sheet, Strip, Flat |
Chromium | 0.4 % Show Material materials with Chromium of 0.4 % | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat |
Copper | 0.3 % Show Material materials with Copper of 0.3 % | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat |
Manganese | 0.5 - 0.8 % Show Material materials with Manganese of 0.5 - 0.8 % | quenched and tempered (+QT) | ISO 683-1, EN 10083-2, EN 10083-1, EN 10083-3 | Bar, Forging, Sheet, Strip, Flat |
Molybdenum | 0.1 % Show Material materials with Molybdenum of 0.1 % | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat |
Nickel | 0.4 % Show Material materials with Nickel of 0.4 % | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat |
Phosphorus | 0.025 % Show Material materials with Phosphorus of 0.025 % | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat |
0.03 % Show Material materials with Phosphorus of 0.03 % | quenched and tempered (+QT) | EN 10083-2, ISO 683-1 | Bar, Forging, Sheet, Strip, Flat | |
0.035 % Show Material materials with Phosphorus of 0.035 % | quenched and tempered (+QT) | EN 10083-1, EN 10083-2, EN 10083-3, ISO 683-1 | Bar, Forging, Sheet, Strip, Flat | |
Silicon | 0.1 - 0.4 % Show Material materials with Silicon of 0.1 - 0.4 % | quenched and tempered (+QT) | ISO 683-1, EN 10083-2 | Bar, Forging, Sheet, Strip, Flat |
0.4 % Show Material materials with Silicon of 0.4 % | quenched and tempered (+QT) | EN 10083-2, ISO 683-1, EN 10083-1, EN 10083-3 | Bar, Forging, Sheet, Strip, Flat | |
Sulfur | 0.035 % Show Material materials with Sulfur of 0.035 % | quenched and tempered (+QT) | ISO 683-1, EN 10083-2, EN 10083-1, EN 10083-3 | Bar, Forging, Sheet, Strip, Flat |
Technological properties
Property | ||
---|---|---|
Supplier Disclaimer | The given information is a rough description and some properties can depend on various factors such as product thickness. Please contact the supplier or refer to the related norm or standard for further information. |