EN 10277-4 Grade 16MnCrB5 soft annealed and peeled (+A+SH)

Want to keep this datasheet? Save it now in your required format

Description

Steel 16MnCrB5 is suitable for predominantly wear loaded parts of favorable ductility behaviour in case hardened condition for vehicle and machine engineering (e.g. piston pins, camshafts). As a bright steel product it is used in the form of bars, bright, straight, in various conditions (see DIN EN 10277 : 1999-10).

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

Properties

General

PropertyTemperatureValueComment

Density

23.0 °C

7.8 - 7.9 g/cm³

Show Material materials with Density of 7.8 - 7.9 g/cm³

Typical for Chromium Steel

Mechanical

PropertyTemperatureValueComment

Elastic modulus

200.0 °C

188 GPa

Show Material materials with Elastic modulus of 188 GPa

Hardness, Brinell

20.0 °C

207 [-]

Show Material materials with Hardness, Brinell of 207 [-]

Poisson's ratio

23.0 °C

0.29 [-]

Show Material materials with Poisson's ratio of 0.29 [-]

Typical for Chromium Steel

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

100.0 °C

1.1E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.1E-5 1/K

Melting point

1382 - 1529 °C

Show Material materials with Melting point of 1382 - 1529 °C

Typical for Chromium Steel

Specific heat capacity

23.0 °C

440 - 494 J/(kg·K)

Show Material materials with Specific heat capacity of 440 - 494 J/(kg·K)

Typical for Chromium Steel

Thermal conductivity

100.0 °C

39.8 W/(m·K)

Show Material materials with Thermal conductivity of 39.8 W/(m·K)

200.0 °C

37.7 W/(m·K)

Show Material materials with Thermal conductivity of 37.7 W/(m·K)

Chemical properties

PropertyValue

Boron

8E-4 - 5E-3 %

Show Material materials with Boron of 8E-4 - 5E-3 %

Carbon

0.14 - 0.19 %

Show Material materials with Carbon of 0.14 - 0.19 %

Chromium

0.8 - 1.1 %

Show Material materials with Chromium of 0.8 - 1.1 %

Manganese

1 - 1.3 %

Show Material materials with Manganese of 1 - 1.3 %

Phosphorus

0.03 - 0.04 %

Show Material materials with Phosphorus of 0.03 - 0.04 %

Silicon

0.4 %

Show Material materials with Silicon of 0.4 %

Sulfur

0.035 %

Show Material materials with Sulfur of 0.035 %