General
Property | Temperature | Value |
---|---|---|
Density | 20.0 °C | 8.85 - 8.9 g/cm³ Show Material materials with Density of 8.85 - 8.9 g/cm³ |
Mechanical
Property | Temperature | Value |
---|---|---|
Elastic modulus | 20.0 °C | 120 GPa Show Material materials with Elastic modulus of 120 GPa |
Hardness, Brinell | 20.0 °C | 80 - 110 [-] Show Material materials with Hardness, Brinell of 80 - 110 [-] |
Hardness, Vickers | 20.0 °C | 85 - 115 [-] Show Material materials with Hardness, Vickers of 85 - 115 [-] |
Poisson's ratio | 20.0 °C | 0.34 [-] Show Material materials with Poisson's ratio of 0.34 [-] |
Thermal
Property | Temperature | Value | Comment |
---|---|---|---|
Coefficient of thermal expansion | 23.0 °C | 1.5E-5 - 1.9E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.5E-5 - 1.9E-5 1/K | Typical for Leaded Phosphor Bronze |
Specific heat capacity | 20.0 °C | 380 J/(kg·K) Show Material materials with Specific heat capacity of 380 J/(kg·K) | |
Thermal conductivity | 20.0 °C | 96 W/(m·K) Show Material materials with Thermal conductivity of 96 W/(m·K) |
Electrical
Property | Temperature | Value |
---|---|---|
Electrical conductivity | 20.0 °C | 1.00E+7 S/m Show Material materials with Electrical conductivity of 1.00E+7 S/m |
Specific Electrical conductivity | 17 % IACS Show Material materials with Specific Electrical conductivity of 17 % IACS |
Chemical properties
Property | Value |
---|---|
Iron | 0.1 % Show Material materials with Iron of 0.1 % |
Lead | 0.02 % Show Material materials with Lead of 0.02 % |
Nickel | 0.2 % Show Material materials with Nickel of 0.2 % |
Phosphorus | 0.01 - 0.4 % Show Material materials with Phosphorus of 0.01 - 0.4 % |
Tin | 4.5 - 5.5 % Show Material materials with Tin of 4.5 - 5.5 % |
Zinc | 0.2 % Show Material materials with Zinc of 0.2 % |