General
Property | Value | Temperature |
---|---|---|
Density | 2.7 g/cm³ Show Material materials with Density of 2.7 g/cm³ at 23.0 °C | 23.0 °C |
Mechanical
Property | Value | Temperature | Comment |
---|---|---|---|
Elastic modulus | 71 GPa Show Material materials with Elastic modulus of 71 GPa at 23.0 °C | 23.0 °C | |
Elongation | 13 % Show Material materials with Elongation of 13 % at 23.0 °C | 23.0 °C | |
Elongation A100 | 10 - 12 % Show Material materials with Elongation A100 of 10 - 12 % at 23.0 °C | 23.0 °C | |
Elongation A50 | 12 - 14 % Show Material materials with Elongation A50 of 12 - 14 % at 23.0 °C | 23.0 °C | |
Plane-Strain Fracture Toughnes | 22 - 35 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22 - 35 MPa·√m at 23.0 °C | 23.0 °C | Typical for Wrought 5000 Series Aluminium |
Poisson's ratio | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] at 23.0 °C | 23.0 °C | Typical for Wrought 5000 Series Aluminium |
Shear modulus | 26 - 26.5 GPa Show Material materials with Shear modulus of 26 - 26.5 GPa at 23.0 °C | 23.0 °C | Typical for Wrought 5000 Series Aluminium |
Tensile strength | 270 - 310 MPa Show Material materials with Tensile strength of 270 - 310 MPa at 23.0 °C | 23.0 °C | |
Yield strength | 150 MPa Show Material materials with Yield strength of 150 MPa at 23.0 °C | 23.0 °C | |
Yield strength Rp0.2 | 110 - 165 MPa Show Material materials with Yield strength Rp0.2 of 110 - 165 MPa at 23.0 °C | 23.0 °C |
Thermal
Property | Value | Temperature | Comment |
---|---|---|---|
Coefficient of thermal expansion | 2.4E-5 1/K Show Material materials with Coefficient of thermal expansion of 2.4E-5 1/K at 23.0 °C | 23.0 °C | |
Max service temperature | 150 °C Show Material materials with Max service temperature of 150 °C | Typical for Wrought 5000 Series Aluminium | |
Melting point | 580 °C Show Material materials with Melting point of 580 °C | ||
Specific heat capacity | 900 J/(kg·K) Show Material materials with Specific heat capacity of 900 J/(kg·K) at 23.0 °C | 23.0 °C | |
Thermal conductivity | 120 W/(m·K) Show Material materials with Thermal conductivity of 120 W/(m·K) at 23.0 °C | 23.0 °C |
Electrical
Property | Value | Temperature | Comment |
---|---|---|---|
Electrical conductivity | 1.80E+7 - 3.10E+7 S/m Show Material materials with Electrical conductivity of 1.80E+7 - 3.10E+7 S/m at 23.0 °C | 23.0 °C | Typical for Wrought 5000 Series Aluminium |
Electrical resistivity | 3.3E-8 - 5E-8 Ω·m Show Material materials with Electrical resistivity of 3.3E-8 - 5E-8 Ω·m at 23.0 °C | 23.0 °C | Typical for Wrought 5000 Series Aluminium |
Chemical properties
Property | ||
---|---|---|
Aluminium | 92.4 - 95.6 % | |
Chromium | 0.05 - 0.25 % | |
Copper | 0 - 0.1 % | |
Iron | 0 - 0.4 % | |
Magnesium | 4 - 4.9 % | |
Manganese | 0.4 - 1 % | |
Other | 0 - 0.15 % | each 0.05, total 0.15, Rest Al |
Silicon | 0 - 0.4 % | |
Titanium | 0 - 0.15 % | |
Zinc | 0 - 0.25 % |
Technological properties
Property | ||
---|---|---|
Brazing | general: no brazing is known or developed | |
Corrosion properties | Stress corrosion cracking: kein Schadensfall im Betrieb und bei Labortests (O, H321, H116), kein Schadensfall im Betrieb, eingeschränkte Schäden bei den Labortests (H111), general: very good, without protection in industrial or seawater atmosphere | |
General machinability | General: poor | |
Workability | general (condition): acceptable (O), poor(H321, H116, H111) |