AA Standards Grade 6082 T6

Want to keep this datasheet? Save it now in your required format

Description

Aluminium alloy 6082 is a medium strength alloy with excellent corrosion resistance. It has the highest strength of the 6000 series alloys. Alloy 6082 is known as a structural alloy. In plate form, 6082 is the alloy most commonly used for machining. As a relatively new alloy, the higher strength of 6082 has seen it replace 6061 in many applications. The addition of a large amount of manganese controls the grain structure which in turn results in a stronger alloy. It is difficult to produce thin walled, complicated extrusion shapes in alloy 6082. The extruded surface finish is not as smooth as other similar strength alloys in the 6000 series. In the T6 and T651 temper, alloy 6082 machines well and produces tight coils of swarf when chip breakers are used.

Related Standards

Equivalent Materials

This material data has been provided by AluKey,MakeItFrom.com,WroughtAl_Thermal,Righton Blackburns.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyValueConditionRelated StandardsShape

Density

2.7 g/cm³

Show Material materials with Density of 2.7 g/cm³

T6

AA Standards, ASTM B221, BS EN 573-3, BS EN 755-2, BS EN 485-2

Bar, Tube, Plate, Sheet

Mechanical

PropertyValueConditionRelated StandardsShapeComment

Elastic modulus

72.0 GPa

Show Material materials with Elastic modulus of 72.0 GPa

T6

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

T6

BS EN 573-3, BS EN 755-2, BS EN 485-2

Bar, Tube, Plate, Sheet

Elongation

6.0 %

Show Material materials with Elongation of 6.0 %

T6

AA Standards, ASTM B221, BS EN 573-3, BS EN 755-2

Bar, Tube

A50

9.0 %

Show Material materials with Elongation of 9.0 %

T6

BS EN 573-3, BS EN 485-2

Plate

A50

8.0 %

Show Material materials with Elongation of 8.0 %

T6

AA Standards, ASTM B221

A100

8.5 %

Show Material materials with Elongation of 8.5 %

T6

6.0 - 10.0 %

Show Material materials with Elongation of 6.0 - 10.0 %

T6

BS EN 573-3, BS EN 755-2

Bar, Tube

Hardness, Brinell

95.0 [-]

Show Material materials with Hardness, Brinell of 95.0 [-]

T6

BS EN 573-3, BS EN 755-2

Bar, Tube

84.0 - 91.0 [-]

Show Material materials with Hardness, Brinell of 84.0 - 91.0 [-]

T6

BS EN 573-3, BS EN 485-2

Plate

94.0 [-]

Show Material materials with Hardness, Brinell of 94.0 [-]

T6

BS EN 573-3, BS EN 485-2

Sheet

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 6000 Series Aluminium

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 6000 Series Aluminium

Shear modulus

26.0 - 26.5 GPa

Show Material materials with Shear modulus of 26.0 - 26.5 GPa

Typical for Wrought 6000 Series Aluminium

Tensile strength

310.0 MPa

Show Material materials with Tensile strength of 310.0 MPa

T6

AA Standards, ASTM B221, BS EN 573-3, BS EN 485-2

Sheet

330.0 MPa

Show Material materials with Tensile strength of 330.0 MPa

T6

270.0 - 310.0 MPa

Show Material materials with Tensile strength of 270.0 - 310.0 MPa

T6

BS EN 573-3, BS EN 755-2

Bar, Tube

275.0 - 300.0 MPa

Show Material materials with Tensile strength of 275.0 - 300.0 MPa

T6

BS EN 573-3, BS EN 485-2

Plate

Yield strength

260.0 MPa

Show Material materials with Yield strength of 260.0 MPa

T6

AA Standards, ASTM B221, BS EN 573-3, BS EN 485-2

Sheet

RP02

200.0 - 260.0 MPa

Show Material materials with Yield strength of 200.0 - 260.0 MPa

T6

BS EN 573-3, BS EN 755-2

Bar, Tube

RP02

240.0 - 255.0 MPa

Show Material materials with Yield strength of 240.0 - 255.0 MPa

T6

BS EN 573-3, BS EN 485-2

Plate

RP02

280.0 MPa

Show Material materials with Yield strength of 280.0 MPa

T6

Thermal

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coefficient of thermal expansion

2.3e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3e-05 1/K

T6

100 °C

0.000022 1/K

Show Material materials with Coefficient of thermal expansion of 0.000022 1/K

T6

unstated value for 20-100°C

2.4e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.4e-05 1/K

T6

BS EN 573-3, BS EN 755-2, BS EN 485-2

Bar, Tube, Plate, Sheet

Melting point

580.0 °C

Show Material materials with Melting point of 580.0 °C

T6

555.0 °C

Show Material materials with Melting point of 555.0 °C

T6

BS EN 573-3, BS EN 755-2, BS EN 485-2

Bar, Tube, Plate, Sheet

Specific heat capacity

890.0 J/(kg·K)

Show Material materials with Specific heat capacity of 890.0 J/(kg·K)

T6

Thermal conductivity

170.0 W/(m·K)

Show Material materials with Thermal conductivity of 170.0 W/(m·K)

T6

180.0 W/(m·K)

Show Material materials with Thermal conductivity of 180.0 W/(m·K)

T6

BS EN 573-3, BS EN 755-2, BS EN 485-2

Bar, Tube, Plate, Sheet

Electrical

PropertyValueConditionRelated StandardsShapeComment

Electrical conductivity

21000000.0 - 34000000.0 S/m

Show Material materials with Electrical conductivity of 21000000.0 - 34000000.0 S/m

Typical for Wrought 6000 Series Aluminium

Electrical resistivity

3.8e-08 Ω·m

Show Material materials with Electrical resistivity of 3.8e-08 Ω·m

T6

BS EN 573-3, BS EN 755-2, BS EN 485-2

Bar, Tube, Plate, Sheet

Chemical properties

PropertyValueConditionRelated StandardsShapeComment

Aluminium

95.2 - 98.3 %

Show Material materials with Aluminium of 95.2 - 98.3 %

T6

Chromium

0.25 %

Show Material materials with Chromium of 0.25 %

T6

AA Standards, ASTM B221, BS EN 573-3, BS EN 755-2, BS EN 485-2

Bar, Tube, Plate, Sheet

Copper

0.1 %

Show Material materials with Copper of 0.1 %

T6

AA Standards, ASTM B221, BS EN 573-3, BS EN 755-2, BS EN 485-2

Bar, Tube, Plate, Sheet

Iron

0.50 %

Show Material materials with Iron of 0.50 %

T6

AA Standards, ASTM B221

0.5 %

Show Material materials with Iron of 0.5 %

T6

BS EN 573-3, BS EN 755-2, BS EN 485-2

Bar, Tube, Plate, Sheet

Magnesium

0.6 - 1.2 %

Show Material materials with Magnesium of 0.6 - 1.2 %

T6

AA Standards, ASTM B221, BS EN 573-3, BS EN 755-2, BS EN 485-2

Bar, Tube, Plate, Sheet

Manganese

0.4 - 1.0 %

Show Material materials with Manganese of 0.4 - 1.0 %

T6

AA Standards, ASTM B221, BS EN 573-3, BS EN 755-2, BS EN 485-2

Bar, Tube, Plate, Sheet

Other

0.15 %

Show Material materials with Other of 0.15 %

T6

BS EN 573-3, BS EN 755-2, BS EN 485-2

Bar, Tube, Plate, Sheet

Total

Silicon

0.7 - 1.3 %

Show Material materials with Silicon of 0.7 - 1.3 %

T6

AA Standards, ASTM B221, BS EN 573-3, BS EN 755-2, BS EN 485-2

Bar, Tube, Plate, Sheet

Titanium

0.1 %

Show Material materials with Titanium of 0.1 %

T6

AA Standards, ASTM B221, BS EN 573-3, BS EN 755-2, BS EN 485-2

Bar, Tube, Plate, Sheet

Zinc

0.2 %

Show Material materials with Zinc of 0.2 %

T6

AA Standards, ASTM B221, BS EN 573-3, BS EN 755-2, BS EN 485-2

Bar, Tube, Plate, Sheet

Technological properties

Property
Application areas

Highly stressed applications, Trusses, Bridges, Cranes, Transport applications, Ore skips, Beer barrels, Milk churns

Brazing

Good

General machinability

Good

Soldering general

Good

Welding

6082 has very good weldability but strength is lowered in the weld zone. When welded to itself, alloy 4043 wire is recommended. If welding 6082 to 7005, then the wire used should be alloy 5356. Gas: Good; Arc: Good; Resistance: Good

Workability

Cold: Good