AM100A T6

Want to keep this datasheet? Save it now in your required format

Ashby charts

See where AM100A T6 falls on the material property chart for Density against Elastic modulus in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

Density

ρ

1.9 g/cm³ at 23 °C

Mechanical

Elastic modulus

E

48 GPa at 23 °C

Show Magnesium materials with Elastic modulus of 48 GPa at 23 °C

Elongation

A

2.3 % at 23 °C

Show Magnesium materials with Elongation of 2.3 % at 23 °C

Poisson's ratio

ν

0.29 [-] at 23 °C

Show Magnesium materials with Poisson's ratio of 0.29 [-] at 23 °C

Typical for Magnesium

Shear modulus

G

45 GPa at 23 °C

Show Magnesium materials with Shear modulus of 45 GPa at 23 °C

Typical for Magnesium

Tensile strength

Rm

270 MPa at 23 °C

Show Magnesium materials with Tensile strength of 270 MPa at 23 °C

Yield strength

YS

120 MPa at 23 °C

Show Magnesium materials with Yield strength of 120 MPa at 23 °C

Thermal

Coefficient of thermal expansion

α

2.5E-5 1/K at 23 °C

Melting point

Tm

460 °C

Specific heat capacity

cp

990 J/(kg·K) at 23 °C

Thermal conductivity

λ

153 - 167 W/(m·K) at 23 °C

Typical for Magnesium

Chemical properties

Element

Weight %

Comment

Mg

87.9 - 90.6 %

Al

9.3 - 10.7 %

Mn

0.1 - 0.35 %

Cu

0 - 0.1 %

Ni

0 - 0.01 %

More

This material data has been provided by MakeItFrom.com.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.