General

Density ρ

3.1 g/cm³ at 20 °C

Mechanical

Elastic modulus E

70 GPa at 20 °C

Elongation A

16 % at 20 °C

Fracture toughness KIC

22 - 35 MPa·√m at 20 °C

Typical for Wrought 2000 Series Aluminium

Poisson's ratio ν

0.33 [-] at 20 °C

Typical for Wrought 2000 Series Aluminium

Shear modulus G

26 - 27.5 GPa at 20 °C

Typical for Wrought 2000 Series Aluminium

Tensile strength Rm

320 MPa at 20 °C

Yield strength YS

140 MPa at 20 °C

Thermal

Coefficient of thermal expansion α

2.3E-5 1/K at 20 °C

Melting point Tm

540 °C

Specific heat capacity cp

860 J/(kg·K) at 20 °C

Thermal conductivity λ

112 - 251 W/(m·K) at 20 °C

Typical for Wrought 2000 Series Aluminium

Electrical

Electrical conductivity σel

1.80E+7 - 3.00E+7 S/m at 20 °C

Typical for Wrought 2000 Series Aluminium

Electrical resistivity ρel

3.4E-8 - 6E-8 Ω·m at 20 °C

Typical for Wrought 2000 Series Aluminium

Chemical properties

Element

Weight %

Comment

Al

91.3 - 94.6 %

Cu

5 - 6 %

Bi

0.2 - 0.6 %

Pb

0.2 - 0.6 %

Fe

0 - 0.7 %

More

Technological properties

Workability

Moderate Workability

This material data has been provided by MakeItFrom.com.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.