Description

Amber neutral glass tubing Acc. to current pharmacopoeias with high chemical resistance, high hydrolytic resistance, UV-block and UV light protection.

This material data has been provided by Schott Glass Tubing.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyValue

Density

2.42 g/cm³

Show Supplier Material materials with Density of 2.42 g/cm³

Mechanical

PropertyValue

Elastic modulus

71 GPa

Show Supplier Material materials with Elastic modulus of 71 GPa

Poisson's ratio

0.19 [-]

Show Supplier Material materials with Poisson's ratio of 0.19 [-]

Thermal

PropertyTemperatureValueTesting StandardComment

Annealing temperature

560.0 °C

Show Supplier Material materials with Annealing temperature of 560.0 °C

ISO 7884-4

Viscosity 10¹³ dPa·s

Coefficient of thermal expansion

5.4e-06 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 5.4e-06 1/K

ISO 7991

mean value for 20-300 °C

Glass transition temperature

550 °C

Show Supplier Material materials with Glass transition temperature of 550 °C

ISO 7884-8

Softening temperature

770.0 °C

Show Supplier Material materials with Softening temperature of 770.0 °C

ISO 7884-3

Viscosity 10⁷·⁶ dPa·s

Specific electrical resistance temperature

200.0 °C

Show Supplier Material materials with Specific electrical resistance temperature of 200.0 °C

For ρ=10⁸ Ω·cm

Thermal conductivity

90 °C

1.2 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 1.2 W/(m·K)

Working temperature

1165.0 °C

Show Supplier Material materials with Working temperature of 1165.0 °C

ISO 7884-2

Viscosity 10⁴ dPa·s

Electrical

PropertyValueFrequency

Dielectric constant

6.3 [-]

Show Supplier Material materials with Dielectric constant of 6.3 [-]

1MHz

Loss tangent

0.0107 [-]

Show Supplier Material materials with Loss tangent of 0.0107 [-]

1MHz

Optical

PropertyValueTesting StandardComment

Refractive index

1.5 [-]

Show Supplier Material materials with Refractive index of 1.5 [-]

at λ=587.6 nm

Stress optical coefficient

2.2e-06 mm²/N

Show Supplier Material materials with Stress optical coefficient of 2.2e-06 mm²/N

DIN 52314

Chemical properties

PropertyValueComment

Aluminium

6 %

Show Supplier Material materials with Aluminium of 6 %

Al₂O₃

Barium

2 %

Show Supplier Material materials with Barium of 2 %

BaO

Boron

7.5 %

Show Supplier Material materials with Boron of 7.5 %

B₂O₃

Calcium

1 %

Show Supplier Material materials with Calcium of 1 %

max. | CaO

Iron

1 %

Show Supplier Material materials with Iron of 1 %

Fe₂O₃

Potassium

1 %

Show Supplier Material materials with Potassium of 1 %

K₂O

Silicon

70 %

Show Supplier Material materials with Silicon of 70 %

SiO₂

Sodium

6.5 %

Show Supplier Material materials with Sodium of 6.5 %

Na₂O

Titanium

5 %

Show Supplier Material materials with Titanium of 5 %

TiO₂

Technological properties

Property
Application areas

Pharmaceutical packaging (Ampoules, Vials, Tablet bottles).

Corrosion properties

Hydrolytic resistance Class HGB1 (ISO 719), Type I (Ph. Eur.), Type I (USP), Fullfield (JP) - Acid resistance Class S1 (DIN 12116) - Alkali resistance Class A2 (ISO695)