Soda Lime Silicate Glass SCHOTT 8516

Alternative and trade names
SCHOTT 8516
Want to keep this datasheet? Save it now in your required format

Description

IR-absorbing sealing glass for Fe-Ni alloys, high IR-absorbing, lead-free and low evaporation.

This material data has been provided by Schott Glass Tubing.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

23.0 °C

2.56 g/cm³

Show Supplier Material materials with Density of 2.56 g/cm³

Mechanical

PropertyTemperatureValue

Elastic modulus

23.0 °C

72 GPa

Show Supplier Material materials with Elastic modulus of 72 GPa

Poisson's ratio

23.0 °C

0.21 [-]

Show Supplier Material materials with Poisson's ratio of 0.21 [-]

Thermal

PropertyTemperatureValueComment

Annealing temperature

445 °C

Show Supplier Material materials with Annealing temperature of 445 °C

Viscosity 10¹³ dPa.s (ISO 7884-4)

Coefficient of thermal expansion

23.0 °C

8.9E-6 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 8.9E-6 1/K

mean value for 20-300 °C - ISO 7991

Glass transition temperature

447 °C

Show Supplier Material materials with Glass transition temperature of 447 °C

ISO 7884-8

Softening temperature

646 °C

Show Supplier Material materials with Softening temperature of 646 °C

Viscosity 10⁷·⁶ dPa.s (ISO 7884-3)

Specific electrical resistance temperature

250 °C

Show Supplier Material materials with Specific electrical resistance temperature of 250 °C

For ρ = 10⁸ Ω·cm

Thermal conductivity

90.0 °C

1.1 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 1.1 W/(m·K)

Working temperature

990 °C

Show Supplier Material materials with Working temperature of 990 °C

Viscosity 10⁴ dPa.s (ISO 7884-2)

Electrical

PropertyTemperatureValue

Dielectric constant, 1MHz

23.0 °C

6.5 [-]

Show Supplier Material materials with Dielectric constant, 1MHz of 6.5 [-]

Electrical resistivity

250.0 °C

1.26E+6 Ω·m

Show Supplier Material materials with Electrical resistivity of 1.26E+6 Ω·m

350.0 °C

25118 Ω·m

Show Supplier Material materials with Electrical resistivity of 25118 Ω·m

Loss tangent, 1MHz

23.0 °C

2.5E-3 [-]

Show Supplier Material materials with Loss tangent, 1MHz of 2.5E-3 [-]

Optical

PropertyValueComment

Refractive index

1.52 [-]

Show Supplier Material materials with Refractive index of 1.52 [-]

at λ=587.6 nm

Stress optical coefficient

3E-6 mm²/N

Show Supplier Material materials with Stress optical coefficient of 3E-6 mm²/N

DIN 52314

Chemical properties

PropertyValueComment

Other

0.01 %

Show Supplier Material materials with Other of 0.01 %

max., Lead, Cadmium, Mercury and Hexavalent Chromium

Technological properties

Property
Application areas

Electronic components (Reed switches and transponders).

Corrosion properties

Hydrolytic resistance Class HGB3 (ISO 719) - Acid resistance Class S1 (DIN 12116) - Alkali resistance Class A2 (ISO695)