Description

The alloy AlZnMgCu1,5 as a Cu-alloyed AlZnMg-alloy achieves highest strength values due to its composition. Strength grade F 55 is achievable by artificial aging. Heat-treatment for hardening: solution annealing: 470 to 480 °C quenching in water artificial aging: 12 to 24 h at 115 to 125 °C 4 to 6 h at 165 to 180 °C The artificial aging represents a two-step aging. Natural aging is unusual. The alloy has a favorable machinability and it is on certain conditions weldable. When welding appears a heat-affected zone of lower strength therefore welding should be avoided. A favorable corrosion resistance can only be warranted for an appropriate surface protection coat. Corrosion resistance can be considerably enhanced by artificial aging. In order to tap the full strength values, without having any negative effect of the lower corrosion resistance, the sheets of this alloy are cladded by rolling with e.g. AlZn1. Therby the application area expands considerably. Furthermore the alloy has a favorable machinability. Application: In machine engineering (incl. mold making) for appliances and tools. Predominantly as anchor, head and punch unit holder plates as well as for guide plates. In mold making esp. in plastics processing for blow, foam and injection forms, carrying constructions for woodworking tools, for machine benchings, turned parts (hydraulics/pneumatics), in vehicle manufacturing for bumper, safety parts. In aircraft construction as connecting elements (screws), in military engineering for bending and forming technics (as wire: springs, screens, hooks etc.).

Related Standards

Equivalent Materials

Ashby charts

See where DIN 1725-1 Grade 3.4365 O falls on the material property chart for Density against Elastic modulus in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

Density

ρ

2.8 g/cm³ at 20 °C

Mechanical

Bulk Modulus

K

72.5 GPa at 20 °C

Show 7000 Series materials with Bulk Modulus of 72.5 GPa at 20 °C

Elastic modulus

E

71 GPa at 20 °C

Show 7000 Series materials with Elastic modulus of 71 GPa at 20 °C

Elongation

A

10 % at 20 °C

Show 7000 Series materials with Elongation of 10 % at 20 °C

Hardness, Brinell

HB

70 [-] at 20 °C

Show 7000 Series materials with Hardness, Brinell of 70 [-] at 20 °C

Plane-Strain Fracture Toughnes

KIC

22 - 35 MPa·√m at 20 °C

Show 7000 Series materials with Plane-Strain Fracture Toughnes of 22 - 35 MPa·√m at 20 °C

Typical for Wrought 7000 Series Aluminium

Poisson's ratio

ν

0.33 [-] at 20 °C

Show 7000 Series materials with Poisson's ratio of 0.33 [-] at 20 °C

Typical for Wrought 7000 Series Aluminium

Shear modulus

G

26.4 - 27.1 GPa at 20 °C

Show 7000 Series materials with Shear modulus of 26.4 - 27.1 GPa at 20 °C

Typical for Wrought 7000 Series Aluminium

Tensile strength

Rm

290 MPa at 20 °C

Show 7000 Series materials with Tensile strength of 290 MPa at 20 °C

Yield strength Rp0.2

Rp0.2

180 MPa at 20 °C

Show 7000 Series materials with Yield strength Rp0.2 of 180 MPa at 20 °C

Thermal

Coefficient of thermal expansion

α

2.1E-5 - 2.4E-5 1/K at 20 °C

Typical for Wrought 7000 Series Aluminium

Specific heat capacity

cp

795 - 1050 J/(kg·K) at 20 °C

Typical for Wrought 7000 Series Aluminium

Thermal conductivity

λ

121 - 170 W/(m·K) at 20 °C

Typical for Wrought 7000 Series Aluminium

Electrical

Electrical conductivity

σel

1.80E+7 - 3.40E+7 S/m at 20 °C

Typical for Wrought 7000 Series Aluminium

Electrical resistivity

ρel

2.9E-8 - 5.6E-8 Ω·m at 20 °C

Typical for Wrought 7000 Series Aluminium

Chemical properties

Element

Weight %

Comment

Zn

5.1 - 6.1 %

Mg

2.1 - 2.9 %

Cu

1.2 - 2 %

Fe

0.5 %

Si

0.4 %

More

Technological properties

Brazing

Excellent

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.