EN 573-1 Grade AW-3105A H24

Want to keep this datasheet? Save it now in your required format

Description

A low to medium strength alloy with good corrosion resistance.

Related Standards

Ashby charts

See where EN 573-1 Grade AW-3105A H24 falls on the material property chart for Density against Elastic modulus in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

Density

ρ

2.71 g/cm³ at 20 °C

Dimension

Dimensions

Dicke

Thickness

t

0.18 - 1 mm

Mechanical

Bending angle 180°

θ180

2.5 °/t at 20 °C

Show 3000 Series materials with Bending angle 180° of 2.5 °/t at 20 °C

Elastic modulus

E

69 GPa at 20 °C

Show 3000 Series materials with Elastic modulus of 69 GPa at 20 °C

Elongation A50

A50

3 % at 20 °C

Show 3000 Series materials with Elongation A50 of 3 % at 20 °C

Hardness, HBW

HBW

48 [-] at 20 °C

Show 3000 Series materials with Hardness, HBW of 48 [-] at 20 °C

Plane-Strain Fracture Toughnes

KIC

22 - 35 MPa·√m at 20 °C

Show 3000 Series materials with Plane-Strain Fracture Toughnes of 22 - 35 MPa·√m at 20 °C

Typical for Wrought 3000 Series Aluminium

Poisson's ratio

ν

0.33 [-] at 20 °C

Show 3000 Series materials with Poisson's ratio of 0.33 [-] at 20 °C

Typical for Wrought 3000 Series Aluminium

Shear modulus

G

26 GPa at 20 °C

Show 3000 Series materials with Shear modulus of 26 GPa at 20 °C

Tensile strength

Rm

150 - 240 MPa at 20 °C

Show 3000 Series materials with Tensile strength of 150 - 240 MPa at 20 °C

Yield strength

YS

120 - 220 MPa at 20 °C

Show 3000 Series materials with Yield strength of 120 - 220 MPa at 20 °C

Yield strength Rp0.2

Rp0.2

120 - 160 MPa at 20 °C

Show 3000 Series materials with Yield strength Rp0.2 of 120 - 160 MPa at 20 °C

Thermal

Coefficient of thermal expansion

α

2.4E-5 1/K at 100 °C

20-100°C

Melting point

Tm

629 - 654 °C

Typical for Wrought 3000 Series Aluminium

Specific heat capacity

cp

893 - 920 J/(kg·K) at 20 °C

Typical for Wrought 3000 Series Aluminium

Thermal conductivity

λ

172 W/(m·K) at 20 °C

Electrical

Electrical conductivity

σel

2.30E+7 - 2.90E+7 S/m at 20 °C

Typical for Wrought 3000 Series Aluminium

Electrical resistivity

ρel

3.8E-8 Ω·m at 20 °C

Chemical properties

Element

Weight %

Comment

Other

-

each 0.05, total 0.15, Rest Al

Fe

0.7 %

Si

0.6 %

Cu

0.3 %

Mn

0.3 - 0.8 %

More

Technological properties

Anodizing

Good

Application areas

Closures: Short cups; Food can: Body, Lids; Semi-rigid and corrugated: Pet food

Brazing

Good

Corrosion properties

Very Good

Welding

Very Good

Workability

Very Good

This material data has been provided by Aludium,WIAM,AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.