Description

Very good corrosion resistance and workability. Very ductile in annealed condition.

Related Standards

Equivalent Materials

Ashby charts

See where EN 573-1 Grade AW-5050 O falls on the material property chart for Density against Elastic modulus in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

Density

ρ

2.68 - 2.69 g/cm³ at 20 °C

Dimension

Dimensions

Dicke

Thickness

t

0.2 - 6 mm

Mechanical

Plane-Strain Fracture Toughnes

KIC

Typical for Wrought 5000 Series Aluminium

Poisson's ratio

ν

Typical for Wrought 5000 Series Aluminium

Tensile strength, transverse

Rm,trans

Yield strength Rp0.2, transverse

Rp0.2,trans

Thermal

Coefficient of thermal expansion

α

2.38E-5 1/K at 20 °C

20-100°C

Hide chart

Max service temperature

Tmax

150 °C

Typical for Wrought 5000 Series Aluminium

Melting point

Tm

620 - 650 °C

Specific heat capacity

cp

879 - 963 J/(kg·K) at 20 °C

Typical for Wrought 5000 Series Aluminium

Thermal conductivity

λ

170 - 193 W/(m·K) at 20 °C

Electrical

Electrical conductivity

σel

2.30E+7 - 2.90E+7 S/m at 20 °C

Electrical resistivity

ρel

3.4E-8 - 4.35E-8 Ω·m at 20 °C

Chemical properties

Element

Weight %

Comment

Other

-

each 0.05, total 0.10, Rest Al

Mg

1.1 - 1.8 %

Fe

0.7 %

Si

0.4 %

Zn

0.25 %

More

Technological properties

Anodizing

Very Good (anodizing quality)

Application areas

Roofing: Single sheet, Sheets for composites/ sandwich Panels; Interiors and ceilings: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels, Decoration; Anodizing quality; Tubes: Industrial tubes, Pipes; Food can: Body, Lids

Brazing

Good

Corrosion properties

Excellent

General machinability

Fair

Welding

Excellent

Workability

Very Good

This material data has been provided by Aludium,WIAM,AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.