EN 573-3 Grade AW-2014A T6

Want to keep this datasheet? Save it now in your required format

Description

The material EN AW-AlCu4SiMg(A) is produced for extruded and drawn components, wire and prewire for mechanical applications. The alloy is used for sheet, strip, forged parts and prematerial. It is not food-safe.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyValueConditionRelated StandardsShape

Density

2.8 g/cm³

Show Material materials with Density of 2.8 g/cm³

T6

EN 573-3, EN 1301, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Bending Fatigue Strength

145.0 MPa

Show Material materials with Bending Fatigue Strength of 145.0 MPa

T6

EN 573-3, EN 1301, EN 754, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

Bending angle 90°

5.0 °/t

Show Material materials with Bending angle 90° of 5.0 °/t

T6

EN 573-3, EN 485

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

6.0 °/t

Show Material materials with Bending angle 90° of 6.0 °/t

T6

EN 573-3, EN 485

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

Elastic modulus

73.0 GPa

Show Material materials with Elastic modulus of 73.0 GPa

T6

EN 573-3, EN 1301, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

Elongation

4.0 %

Show Material materials with Elongation of 4.0 %

T6

EN 573-3, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

A50

4.0 %

Show Material materials with Elongation of 4.0 %

T6

EN 573-3, EN 485

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

A100

5.0 %

Show Material materials with Elongation of 5.0 %

T6

EN 573-3, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

A50

5.0 %

Show Material materials with Elongation of 5.0 %

T6

EN 573-3, EN 485, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

A100

6.0 %

Show Material materials with Elongation of 6.0 %

T6

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

A50

6.0 %

Show Material materials with Elongation of 6.0 %

T6

EN 573-3, EN 485, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

A100

7.0 %

Show Material materials with Elongation of 7.0 %

T6

EN 573-3, EN 485

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

A50

7.0 %

Show Material materials with Elongation of 7.0 %

T6

EN 573-3, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

A100

8.0 %

Show Material materials with Elongation of 8.0 %

T6

EN 573-3, EN 485

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

A50

8.0 %

Show Material materials with Elongation of 8.0 %

T6

EN 573-3, EN 754

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

A100

9.0 %

Show Material materials with Elongation of 9.0 %

T6

EN 573-3, EN 1301

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

20.0 °C

4.0 %

Show Material materials with Elongation of 4.0 %

T6

EN 573-3

Tube

A50

20.0 °C

4.0 %

Show Material materials with Elongation of 4.0 %

T6

EN 573-3

Flat

20.0 °C

4.0 %

Show Material materials with Elongation of 4.0 %

T6

EN 573-3

Flat

Transverse

20.0 °C

5.0 %

Show Material materials with Elongation of 5.0 %

T6

EN 573-3

Rod, Tube, Profile

A50

20.0 °C

5.0 %

Show Material materials with Elongation of 5.0 %

T6

EN 573-3

Rod, Flat

20.0 °C

5.0 %

Show Material materials with Elongation of 5.0 %

T6

EN 573-3

Flat

Transverse

20.0 °C

6.0 %

Show Material materials with Elongation of 6.0 %

T6

EN 573-3

Rod, Tube, Flat

A50

20.0 °C

6.0 %

Show Material materials with Elongation of 6.0 %

T6

EN 573-3

Rod, Tube, Flat

20.0 °C

6.0 %

Show Material materials with Elongation of 6.0 %

T6

EN 573-3

Flat

A50 Transverse

20.0 °C

6.0 %

Show Material materials with Elongation of 6.0 %

T6

EN 573-3

Flat

Transverse

20.0 °C

7.0 %

Show Material materials with Elongation of 7.0 %

T6

EN 573-3

Flat

A50

20.0 °C

7.0 %

Show Material materials with Elongation of 7.0 %

T6

EN 573-3

Rod, Tube, Profile

20.0 °C

7.0 %

Show Material materials with Elongation of 7.0 %

T6

EN 573-3

Flat

A50 Transverse

20.0 °C

8.0 %

Show Material materials with Elongation of 8.0 %

T6

EN 573-3

Flat

A50

20.0 °C

8.0 %

Show Material materials with Elongation of 8.0 %

T6

EN 573-3

Rod, Tube

20.0 °C

8.0 %

Show Material materials with Elongation of 8.0 %

T6

EN 573-3

Flat

A50 Transverse

20.0 °C

9.0 %

Show Material materials with Elongation of 9.0 %

T6

EN 573-3

Wire

A100

Hardness, Brinell

150.0 [-]

Show Material materials with Hardness, Brinell of 150.0 [-]

T6

EN 573-3, EN 485

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

20.0 °C

140.0 [-]

Show Material materials with Hardness, Brinell of 140.0 [-]

T6

EN 573-3

Profile, Rod, Tube

20.0 °C

150.0 [-]

Show Material materials with Hardness, Brinell of 150.0 [-]

T6

EN 573-3

Flat

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 2000 Series Aluminium

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 2000 Series Aluminium

Shear modulus

27.4 GPa

Show Material materials with Shear modulus of 27.4 GPa

T6

EN 573-3, EN 1301, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

Tensile strength

410.0 MPa

Show Material materials with Tensile strength of 410.0 MPa

T6

EN 573-3, EN 485

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

415.0 MPa

Show Material materials with Tensile strength of 415.0 MPa

T6

EN 573-3, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

420.0 MPa

Show Material materials with Tensile strength of 420.0 MPa

T6

EN 573-3, EN 485, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

430.0 MPa

Show Material materials with Tensile strength of 430.0 MPa

T6

EN 573-3, EN 485, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

440.0 MPa

Show Material materials with Tensile strength of 440.0 MPa

T6

EN 573-3, EN 1301, EN 485

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

450.0 MPa

Show Material materials with Tensile strength of 450.0 MPa

T6

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

460.0 MPa

Show Material materials with Tensile strength of 460.0 MPa

T6

EN 573-3, EN 485, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

465.0 MPa

Show Material materials with Tensile strength of 465.0 MPa

T6

EN 573-3, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

20.0 °C

410.0 MPa

Show Material materials with Tensile strength of 410.0 MPa

T6

EN 573-3

Flat

20.0 °C

410.0 MPa

Show Material materials with Tensile strength of 410.0 MPa

T6

EN 573-3

Flat

Transverse

20.0 °C

415.0 MPa

Show Material materials with Tensile strength of 415.0 MPa

T6

EN 573-3

Rod, Tube, Profile

20.0 °C

420.0 MPa

Show Material materials with Tensile strength of 420.0 MPa

T6

EN 573-3

Rod, Flat

20.0 °C

420.0 MPa

Show Material materials with Tensile strength of 420.0 MPa

T6

EN 573-3

Flat

Transverse

20.0 °C

430.0 MPa

Show Material materials with Tensile strength of 430.0 MPa

T6

EN 573-3

Rod, Flat

20.0 °C

430.0 MPa

Show Material materials with Tensile strength of 430.0 MPa

T6

EN 573-3

Flat

Transverse

20.0 °C

440.0 MPa

Show Material materials with Tensile strength of 440.0 MPa

T6

EN 573-3

Wire, Flat

20.0 °C

440.0 MPa

Show Material materials with Tensile strength of 440.0 MPa

T6

EN 573-3

Flat

Transverse

20.0 °C

450.0 MPa

Show Material materials with Tensile strength of 450.0 MPa

T6

EN 573-3

Rod, Tube, Flat

20.0 °C

450.0 MPa

Show Material materials with Tensile strength of 450.0 MPa

T6

EN 573-3

Flat

Transverse

20.0 °C

460.0 MPa

Show Material materials with Tensile strength of 460.0 MPa

T6

EN 573-3

Rod, Flat, Profile

20.0 °C

460.0 MPa

Show Material materials with Tensile strength of 460.0 MPa

T6

EN 573-3

Flat

Transverse

20.0 °C

465.0 MPa

Show Material materials with Tensile strength of 465.0 MPa

T6

EN 573-3

Rod

Thermal

PropertyValueComment

Coefficient of thermal expansion

1.6e-05 - 2.4e-05 1/K

Show Material materials with Coefficient of thermal expansion of 1.6e-05 - 2.4e-05 1/K

Typical for Wrought 2000 Series Aluminium

Melting point

500.0 - 650.0 °C

Show Material materials with Melting point of 500.0 - 650.0 °C

Typical for Wrought 2000 Series Aluminium

Specific heat capacity

816.0 - 963.0 J/(kg·K)

Show Material materials with Specific heat capacity of 816.0 - 963.0 J/(kg·K)

Typical for Wrought 2000 Series Aluminium

Thermal conductivity

112.0 - 251.0 W/(m·K)

Show Material materials with Thermal conductivity of 112.0 - 251.0 W/(m·K)

Typical for Wrought 2000 Series Aluminium

Electrical

PropertyValueComment

Electrical conductivity

18000000.0 - 30000000.0 S/m

Show Material materials with Electrical conductivity of 18000000.0 - 30000000.0 S/m

Typical for Wrought 2000 Series Aluminium

Electrical resistivity

3.4e-08 - 6e-08 Ω·m

Show Material materials with Electrical resistivity of 3.4e-08 - 6e-08 Ω·m

Typical for Wrought 2000 Series Aluminium

Chemical properties

PropertyValueConditionRelated StandardsShape

Beryllium

0.0001 - 0.005 %

Show Material materials with Beryllium of 0.0001 - 0.005 %

T6

EN 573-3, EN 1301, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

Chromium

0.1 %

Show Material materials with Chromium of 0.1 %

T6

EN 573-3, EN 1301, EN 485, EN 754, EN 755

Rod, Flat, Tube, Profile, Wire, Strip, Sheet, Plate, Welded Tube

Copper

3.9 - 5.0 %

Show Material materials with Copper of 3.9 - 5.0 %

T6

EN 573-3, EN 1301, EN 485, EN 754, EN 755

Rod, Flat, Tube, Profile, Wire, Strip, Sheet, Plate, Welded Tube

Iron

0.5 %

Show Material materials with Iron of 0.5 %

T6

EN 573-3

Rod, Flat, Tube, Profile, Wire

0.50 %

Show Material materials with Iron of 0.50 %

T6

EN 573-3, EN 1301, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

Magnesium

0.2 - 0.8 %

Show Material materials with Magnesium of 0.2 - 0.8 %

T6

EN 573-3, EN 1301, EN 485, EN 754, EN 755

Rod, Flat, Tube, Profile, Wire, Strip, Sheet, Plate, Welded Tube

Manganese

0.4 - 1.2 %

Show Material materials with Manganese of 0.4 - 1.2 %

T6

EN 573-3, EN 1301, EN 485, EN 754, EN 755

Rod, Flat, Tube, Profile, Wire, Strip, Sheet, Plate, Welded Tube

Nickel

0.1 %

Show Material materials with Nickel of 0.1 %

T6

EN 573-3, EN 1301, EN 485, EN 754, EN 755

Rod, Flat, Tube, Profile, Wire, Strip, Sheet, Plate, Welded Tube

Silicon

0.5 - 0.9 %

Show Material materials with Silicon of 0.5 - 0.9 %

T6

EN 573-3, EN 1301, EN 485, EN 754, EN 755

Rod, Flat, Tube, Profile, Wire, Strip, Sheet, Plate, Welded Tube

Titanium

0.15 %

Show Material materials with Titanium of 0.15 %

T6

EN 573-3, EN 1301, EN 485, EN 754, EN 755

Rod, Flat, Tube, Profile, Wire, Strip, Sheet, Plate, Welded Tube

Zinc

0.25 %

Show Material materials with Zinc of 0.25 %

T6

EN 573-3, EN 1301, EN 485, EN 754, EN 755

Rod, Flat, Tube, Profile, Wire, Strip, Sheet, Plate, Welded Tube

Technological properties

Property
Workability

Moderate Workability