General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Density | 2.77 g/cm³ Show Material materials with Density of 2.77 g/cm³ | H18 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |
20.0 °C | 2.77 g/cm³ Show Material materials with Density of 2.77 g/cm³ | H18 | EN 573-3 | Wire |
Mechanical
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Elastic modulus | 73.0 GPa Show Material materials with Elastic modulus of 73.0 GPa | H18 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | ||
20.0 °C | 70.0 - 74.5 GPa Show Material materials with Elastic modulus of 70.0 - 74.5 GPa | H18 | EN 573-3 | Wire | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 2000 Series Aluminium | ||||
Poisson's ratio | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] | Typical for Wrought 2000 Series Aluminium | ||||
Shear modulus | 27.4 GPa Show Material materials with Shear modulus of 27.4 GPa | H18 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | ||
20.0 °C | 27.0 - 28.0 GPa Show Material materials with Shear modulus of 27.0 - 28.0 GPa | H18 | EN 573-3 | Wire | ||
Tensile strength | 320.0 MPa Show Material materials with Tensile strength of 320.0 MPa | H18 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | ||
20.0 °C | 320.0 MPa Show Material materials with Tensile strength of 320.0 MPa | H18 | EN 573-3 | Wire |
Thermal
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Coefficient of thermal expansion | -50 °C | 2.11e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.11e-05 1/K | H18 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar |
20 °C | 2.11e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.11e-05 1/K | H18 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |
20 °C | 2.2899999999999998e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.2899999999999998e-05 1/K | H18 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |
20 °C | 2.3199999999999998e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.3199999999999998e-05 1/K | H18 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |
20 °C | 2.38e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.38e-05 1/K | H18 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |
20 °C | 2.4699999999999997e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.4699999999999997e-05 1/K | H18 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |
100 °C | 2.2899999999999998e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.2899999999999998e-05 1/K | H18 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |
100 °C | 2.3199999999999998e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.3199999999999998e-05 1/K | H18 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |
200 °C | 2.38e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.38e-05 1/K | H18 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |
300 °C | 2.4699999999999997e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.4699999999999997e-05 1/K | H18 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |
Melting point | 505.0 - 640.0 °C Show Material materials with Melting point of 505.0 - 640.0 °C | H18 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |
505.0 - 635.0 °C Show Material materials with Melting point of 505.0 - 635.0 °C | H18 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | ||
Specific heat capacity | 875.0 J/(kg·K) Show Material materials with Specific heat capacity of 875.0 J/(kg·K) | H18 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |
20.0 °C | 875.0 J/(kg·K) Show Material materials with Specific heat capacity of 875.0 J/(kg·K) | H18 | EN 573-3 | Wire | |
Thermal conductivity | 121.0 - 193.0 W/(m·K) Show Material materials with Thermal conductivity of 121.0 - 193.0 W/(m·K) | H18 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |
20.0 °C | 130.0 - 150.0 W/(m·K) Show Material materials with Thermal conductivity of 130.0 - 150.0 W/(m·K) | H18 | EN 573-3, EN 1301 | Wire, Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar |
Electrical
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Electrical conductivity | 17000000.0 - 29000000.0 S/m Show Material materials with Electrical conductivity of 17000000.0 - 29000000.0 S/m | H18 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |
20.0 °C | 18000000.0 - 21000000.0 S/m Show Material materials with Electrical conductivity of 18000000.0 - 21000000.0 S/m | H18 | EN 573-3, EN 1301 | Wire, Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |
Electrical resistivity | 3.45e-08 - 5.88e-08 Ω·m Show Material materials with Electrical resistivity of 3.45e-08 - 5.88e-08 Ω·m | H18 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |
4.76e-08 - 5.56e-08 Ω·m Show Material materials with Electrical resistivity of 4.76e-08 - 5.56e-08 Ω·m | H18 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chromium | 0.1 % Show Material materials with Chromium of 0.1 % | H18 | EN 573-3, EN 1301 | Wire, Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar |
Copper | 3.8 - 4.9 % Show Material materials with Copper of 3.8 - 4.9 % | H18 | EN 573-3, EN 1301 | Wire, Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar |
Iron | 0.5 % Show Material materials with Iron of 0.5 % | H18 | EN 573-3 | Wire |
0.50 % Show Material materials with Iron of 0.50 % | H18 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |
Magnesium | 1.2 - 1.8 % Show Material materials with Magnesium of 1.2 - 1.8 % | H18 | EN 573-3, EN 1301 | Wire, Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar |
Manganese | 0.3 - 0.9 % Show Material materials with Manganese of 0.3 - 0.9 % | H18 | EN 573-3, EN 1301 | Wire, Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar |
Silicon | 0.5 % Show Material materials with Silicon of 0.5 % | H18 | EN 573-3, EN 1301 | Wire, Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar |
Titanium | 0.15 % Show Material materials with Titanium of 0.15 % | H18 | EN 573-3, EN 1301 | Wire, Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar |
Zinc | 0.25 % Show Material materials with Zinc of 0.25 % | H18 | EN 573-3, EN 1301 | Wire, Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: not suitable, Protective: good | |
Brazing | hard brazing (with flux/ without flux): not suitable / not suitable, friction soldering: acceptable, soft brazing with flux: not suitable | |
Corrosion properties | Seawater: poor, weathering: poor | |
Workability | Bending / Spinning (cold): sufficient (O) / acceptable (O), Impact extrusion (cold): acceptable (O), Deep drawing / upsetting (Condition) acceptable (O) / sufficient (O) |