Properties

Electrical

PropertyTemperatureValue

Electrical conductivity

20.0 °C

9.40E+6 S/m

Show Material materials with Electrical conductivity of 9.40E+6 S/m

Electrical resistivity

0.0 °C

9.82E-8 Ω·m

Show Material materials with Electrical resistivity of 9.82E-8 Ω·m

20.0 °C

1.07E-7 - 1.16E-7 Ω·m

Show Material materials with Electrical resistivity of 1.07E-7 - 1.16E-7 Ω·m

General

PropertyTemperatureValue

Density

20.0 °C

21.5 g/cm³

Show Material materials with Density of 21.5 g/cm³

Mechanical

PropertyTemperatureValue

Elastic modulus

-195.0 °C

178 GPa

Show Material materials with Elastic modulus of 178 GPa

20.0 °C

170 - 173 GPa

Show Material materials with Elastic modulus of 170 - 173 GPa

250.0 °C

169 GPa

Show Material materials with Elastic modulus of 169 GPa

400.0 °C

163 GPa

Show Material materials with Elastic modulus of 163 GPa

500.0 °C

159 GPa

Show Material materials with Elastic modulus of 159 GPa

600.0 °C

153 GPa

Show Material materials with Elastic modulus of 153 GPa

750.0 °C

140 GPa

Show Material materials with Elastic modulus of 140 GPa

800.0 °C

136 GPa

Show Material materials with Elastic modulus of 136 GPa

900.0 °C

126 GPa

Show Material materials with Elastic modulus of 126 GPa

1000.0 °C

115 GPa

Show Material materials with Elastic modulus of 115 GPa

Unlock all property charts

Elongation

20.0 °C

28 - 65 %

Show Material materials with Elongation of 28 - 65 %

Reduction of area

20.0 °C

99 %

Show Material materials with Reduction of area of 99 %

Tensile strength

20.0 °C

9 - 168 MPa

Show Material materials with Tensile strength of 9 - 168 MPa

Yield strength Rp0.2

20.0 °C

30 - 105 MPa

Show Material materials with Yield strength Rp0.2 of 30 - 105 MPa

Thermal

PropertyTemperatureValue

Coefficient of thermal expansion

100.0 °C

9.1E-6 1/K

Show Material materials with Coefficient of thermal expansion of 9.1E-6 1/K

200.0 °C

9.2E-6 1/K

Show Material materials with Coefficient of thermal expansion of 9.2E-6 1/K

300.0 °C

9.3E-6 1/K

Show Material materials with Coefficient of thermal expansion of 9.3E-6 1/K

400.0 °C

9.5E-6 1/K

Show Material materials with Coefficient of thermal expansion of 9.5E-6 1/K

500.0 °C

9.6E-6 1/K

Show Material materials with Coefficient of thermal expansion of 9.6E-6 1/K

600.0 °C

9.7E-6 1/K

Show Material materials with Coefficient of thermal expansion of 9.7E-6 1/K

700.0 °C

9.9E-6 1/K

Show Material materials with Coefficient of thermal expansion of 9.9E-6 1/K

800.0 °C

1E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1E-5 1/K

900.0 °C

1.01E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.01E-5 1/K

1000.0 °C

1.03E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.03E-5 1/K

1100.0 °C

1.05E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.05E-5 1/K

1200.0 °C

1.06E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.06E-5 1/K

1300.0 °C

1.08E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.08E-5 1/K

1400.0 °C

1.1E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.1E-5 1/K

1500.0 °C

1.12E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.12E-5 1/K

1600.0 °C

1.14E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.14E-5 1/K

Unlock all property charts

Thermal conductivity

-173.0 °C

85.6 W/(m·K)

Show Material materials with Thermal conductivity of 85.6 W/(m·K)

-73.0 °C

79 W/(m·K)

Show Material materials with Thermal conductivity of 79 W/(m·K)

0.0 °C

75 W/(m·K)

Show Material materials with Thermal conductivity of 75 W/(m·K)

20.0 °C

74 W/(m·K)

Show Material materials with Thermal conductivity of 74 W/(m·K)

127.0 °C

73.2 W/(m·K)

Show Material materials with Thermal conductivity of 73.2 W/(m·K)

327.0 °C

73 W/(m·K)

Show Material materials with Thermal conductivity of 73 W/(m·K)

527.0 °C

74.8 W/(m·K)

Show Material materials with Thermal conductivity of 74.8 W/(m·K)

727.0 °C

76.9 W/(m·K)

Show Material materials with Thermal conductivity of 76.9 W/(m·K)

927.0 °C

83.2 W/(m·K)

Show Material materials with Thermal conductivity of 83.2 W/(m·K)

1127.0 °C

88.3 W/(m·K)

Show Material materials with Thermal conductivity of 88.3 W/(m·K)

1327.0 °C

89.5 W/(m·K)

Show Material materials with Thermal conductivity of 89.5 W/(m·K)

1527.0 °C

89 W/(m·K)

Show Material materials with Thermal conductivity of 89 W/(m·K)

1727.0 °C

86 W/(m·K)

Show Material materials with Thermal conductivity of 86 W/(m·K)

Unlock all property charts

Chemical properties

PropertyValue

Platinum

99.5 - 99.99 %