Allgemein
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 2.7 g/cm³ Show Material materials with Dichte of 2.7 g/cm³ | H34 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Plate, Sheet, Strip | |
2.71 g/cm³ Show Material materials with Dichte of 2.71 g/cm³ | H34 | EN 573-3, EN 1592, EN 485 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | ||
20.0 °C | 2.71 g/cm³ Show Material materials with Dichte of 2.71 g/cm³ | H34 | EN 573-3 | Flat |
Abmessung
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Biegewinkel 180° | 2.5 °/t Show Material materials with Biegewinkel 180° of 2.5 °/t | H34 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | ||
2.5 °/t Show Material materials with Biegewinkel 180° of 2.5 °/t | H34 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Plate, Sheet, Strip | |||
Biegewinkel 90° | 1.0 °/t Show Material materials with Biegewinkel 90° of 1.0 °/t | H34 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | ||
1 °/t Show Material materials with Biegewinkel 90° of 1 °/t | H34 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Plate, Sheet, Strip | |||
1.5 °/t Show Material materials with Biegewinkel 90° of 1.5 °/t | H34 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | |||
2.0 °/t Show Material materials with Biegewinkel 90° of 2.0 °/t | H34 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | |||
2.5 °/t Show Material materials with Biegewinkel 90° of 2.5 °/t | H34 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | |||
3.0 °/t Show Material materials with Biegewinkel 90° of 3.0 °/t | H34 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | |||
Dehnung | 6.0 % Show Material materials with Dehnung of 6.0 % | H34 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | A50 | |
6.0 - 8.0 % Show Material materials with Dehnung of 6.0 - 8.0 % | H34 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Plate, Sheet, Strip | A50 | ||
7.0 % Show Material materials with Dehnung of 7.0 % | H34 | EN 573-3, EN 1592 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | A100 | ||
7.0 % Show Material materials with Dehnung of 7.0 % | H34 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | A50 | ||
8.0 % Show Material materials with Dehnung of 8.0 % | H34 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | A100 | ||
8.0 % Show Material materials with Dehnung of 8.0 % | H34 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | A50 | ||
10.0 % Show Material materials with Dehnung of 10.0 % | H34 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | A50 | ||
20.0 °C | 6.0 % Show Material materials with Dehnung of 6.0 % | H34 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 6.0 % Show Material materials with Dehnung of 6.0 % | H34 | EN 573-3 | Flat | A50 | |
20.0 °C | 7.0 % Show Material materials with Dehnung of 7.0 % | H34 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 7.0 % Show Material materials with Dehnung of 7.0 % | H34 | EN 573-3 | Flat | A50 | |
20.0 °C | 8.0 % Show Material materials with Dehnung of 8.0 % | H34 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 8.0 % Show Material materials with Dehnung of 8.0 % | H34 | EN 573-3 | Flat | Transverse | |
20.0 °C | 8.0 % Show Material materials with Dehnung of 8.0 % | H34 | EN 573-3 | Flat | A50 | |
20.0 °C | 8.0 % Show Material materials with Dehnung of 8.0 % | H34 | EN 573-3 | Flat | ||
20.0 °C | 10.0 % Show Material materials with Dehnung of 10.0 % | H34 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 10.0 % Show Material materials with Dehnung of 10.0 % | H34 | EN 573-3 | Flat | A50 | |
Elastizitätsmodul | -270.0 °C | 70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | H34 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 573-3 | Plate, Sheet, Strip, Flat | |
70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | H34 | EN 573-3, EN 1592, EN 485 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | |||
20.0 °C | 70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | H34 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 573-3 | Plate, Sheet, Strip, Flat | ||
50.0 °C | 69.0 GPa Show Material materials with Elastizitätsmodul of 69.0 GPa | H34 | EN 573-3 | Flat | ||
100.0 °C | 68.0 GPa Show Material materials with Elastizitätsmodul of 68.0 GPa | H34 | EN 573-3 | Flat | ||
150.0 °C | 66.0 GPa Show Material materials with Elastizitätsmodul of 66.0 GPa | H34 | EN 573-3 | Flat | ||
200.0 °C | 63.0 GPa Show Material materials with Elastizitätsmodul of 63.0 GPa | H34 | EN 573-3 | Flat | ||
250.0 °C | 57.0 GPa Show Material materials with Elastizitätsmodul of 57.0 GPa | H34 | EN 573-3 | Flat | ||
300.0 °C | 50.0 GPa Show Material materials with Elastizitätsmodul of 50.0 GPa | H34 | EN 573-3 | Flat | ||
Härte, Brinell | 70.0 [-] Show Material materials with Härte, Brinell of 70.0 [-] | H34 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | ||
20.0 °C | 63.0 [-] Show Material materials with Härte, Brinell of 63.0 [-] | H34 | EN 573-3 | Flat | ||
20.0 °C | 63.0 - 70.0 [-] Show Material materials with Härte, Brinell of 63.0 - 70.0 [-] | H34 | EN 573-3 | Flat | ||
20.0 °C | 70.0 [-] Show Material materials with Härte, Brinell of 70.0 [-] | H34 | EN 573-3 | Flat | ||
Härte, HBW | 70 [-] Show Material materials with Härte, HBW of 70 [-] | H34 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Plate, Sheet, Strip | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 5000 Series Aluminium | ||||
Schubmodule | 20.0 °C | 26.5 GPa Show Material materials with Schubmodule of 26.5 GPa | H34 | EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Flat, Plate, Sheet, Strip | |
Streckgrenze | 160.0 MPa Show Material materials with Streckgrenze of 160.0 MPa | H34 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | RP02 | |
160 MPa Show Material materials with Streckgrenze of 160 MPa | H34 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Plate, Sheet, Strip | |||
170.0 MPa Show Material materials with Streckgrenze of 170.0 MPa | H34 | EN 573-3, EN 1592 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | RP02 | ||
20.0 °C | 160.0 MPa Show Material materials with Streckgrenze of 160.0 MPa | H34 | EN 573-3 | Flat | RP02 Transverse | |
20.0 °C | 160.0 MPa Show Material materials with Streckgrenze of 160.0 MPa | H34 | EN 573-3 | Flat | RP02 | |
Zugfestigkeit | 220.0 MPa Show Material materials with Zugfestigkeit of 220.0 MPa | H34 | EN 573-3, EN 1592 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | ||
20.0 °C | 240.0 - 280.0 MPa Show Material materials with Zugfestigkeit of 240.0 - 280.0 MPa | H34 | EN 573-3 | Flat | Transverse | |
20.0 °C | 240.0 - 280.0 MPa Show Material materials with Zugfestigkeit of 240.0 - 280.0 MPa | H34 | EN 573-3, EN 485, EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Strip, Sheet, Plate, Rod, Tube, Welded Tube, Sheet, Strip, Flat |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 20 °C | 2.3699999999999997e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3699999999999997e-05 1/K | H34 | EN 573-3, EN 1592, EN 485 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | |
100 °C | 2.3699999999999997e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3699999999999997e-05 1/K | H34 | EN 573-3, EN 1592, EN 485 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | ||
100 °C | 0.000024 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 0.000024 1/K | H34 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Plate, Sheet, Strip | 20-100°C | |
Max. Betriebstemperatur | 150.0 °C Show Material materials with Max. Betriebstemperatur of 150.0 °C | H34 | EN 573-3 | Flat | Long | |
150.0 °C Show Material materials with Max. Betriebstemperatur of 150.0 °C | Typical for Wrought 5000 Series Aluminium | |||||
Schmelzpunkt | 620.0 - 650.0 °C Show Material materials with Schmelzpunkt of 620.0 - 650.0 °C | H34 | EN 573-3, EN 1592, EN 485 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | ||
Spezifische Wärmekapazität | 879.0 - 963.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 879.0 - 963.0 J/(kg·K) | Typical for Wrought 5000 Series Aluminium | ||||
Wärmeleitfähigkeit | 147 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 147 W/(m·K) | H34 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Plate, Sheet, Strip | ||
20.0 °C | 140.0 - 180.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 140.0 - 180.0 W/(m·K) | H34 | EN 573-3, EN 1592, EN 485 | Flat, Strip, Sheet, Plate, Rod, Tube, Welded Tube |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Elektrische Leitfähigkeit | 20.0 °C | 20000000.0 - 25000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 20000000.0 - 25000000.0 S/m | H34 | EN 573-3, EN 1592, EN 485 | Flat, Strip, Sheet, Plate, Rod, Tube, Welded Tube |
spezifischer Widerstand | 4e-08 - 5e-08 Ω·m Show Material materials with spezifischer Widerstand of 4e-08 - 5e-08 Ω·m | H34 | EN 573-3, EN 1592, EN 485 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | |
4.4e-08 - 5e-08 Ω·m Show Material materials with spezifischer Widerstand of 4.4e-08 - 5e-08 Ω·m | H34 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Plate, Sheet, Strip |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Andere | 0.05 - 0.15 % Show Material materials with Andere of 0.05 - 0.15 % | H34 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Plate, Sheet, Strip |
Chrom | 0.3 % Show Material materials with Chrom of 0.3 % | H34 | EN 573-3, EN 1592, EN 485 | Flat, Strip, Sheet, Plate, Rod, Tube, Welded Tube |
0.3 % Show Material materials with Chrom of 0.3 % | H34 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Plate, Sheet, Strip | |
Eisen | 0.5 % Show Material materials with Eisen of 0.5 % | H34 | EN 573-3 | Flat |
0.50 % Show Material materials with Eisen of 0.50 % | H34 | EN 573-3, EN 1592, EN 485 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | |
0.5 % Show Material materials with Eisen of 0.5 % | H34 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Plate, Sheet, Strip | |
Kupfer | 0.1 % Show Material materials with Kupfer of 0.1 % | H34 | EN 573-3, EN 1592, EN 485 | Flat, Strip, Sheet, Plate, Rod, Tube, Welded Tube |
0.1 % Show Material materials with Kupfer of 0.1 % | H34 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Plate, Sheet, Strip | |
Magnesium | 1.6 - 2.5 % Show Material materials with Magnesium of 1.6 - 2.5 % | H34 | EN 573-3, EN 1592, EN 485, EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Flat, Strip, Sheet, Plate, Rod, Tube, Welded Tube, Sheet, Strip |
Mangan | 0.5 - 1.1 % Show Material materials with Mangan of 0.5 - 1.1 % | H34 | EN 573-3, EN 1592, EN 485, EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Flat, Strip, Sheet, Plate, Rod, Tube, Welded Tube, Sheet, Strip |
Silizium | 0.4 % Show Material materials with Silizium of 0.4 % | H34 | EN 573-3, EN 1592, EN 485 | Flat, Strip, Sheet, Plate, Rod, Tube, Welded Tube |
0.4 % Show Material materials with Silizium of 0.4 % | H34 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Plate, Sheet, Strip | |
Titan | 0.1 % Show Material materials with Titan of 0.1 % | H34 | EN 573-3, EN 1592, EN 485 | Flat, Strip, Sheet, Plate, Rod, Tube, Welded Tube |
0.1 % Show Material materials with Titan of 0.1 % | H34 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Plate, Sheet, Strip | |
Zink | 0.2 % Show Material materials with Zink of 0.2 % | H34 | EN 573-3, EN 1592, EN 485 | Flat, Strip, Sheet, Plate, Rod, Tube, Welded Tube |
0.2 % Show Material materials with Zink of 0.2 % | H34 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Plate, Sheet, Strip |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: sufficient, Protective: good | |
Application areas | Components: General trasportation | |
Brazing | hard brazing (with flux/ without flux): poor / sufficient, friction soldering: acceptable, soft brazing with flux: poor | |
Corrosion properties | Seawater: very good, weathering: very good | |
Welding | Very Good | |
Workability | Bending / Spinning (cold): good / acceptable, Impact extrusion (cold): sufficient, Deep drawing / upsetting (Condition) good (O) / good (H12) |