Allgemein
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 2.68 g/cm³ Show Material materials with Dichte of 2.68 g/cm³ | F | EN 573-3, EN 1386, EN 1715-3, EN 485, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |
20.0 °C | 2.68 g/cm³ Show Material materials with Dichte of 2.68 g/cm³ | F | EN 573-3 | Profile, Rod, Flat, Tube, Plate | |
20.0 °C | 2.68 - 2.69 g/cm³ Show Material materials with Dichte of 2.68 - 2.69 g/cm³ | F | EN 573-3 | Profile, Rod, Flat, Tube, Plate | |
20.0 °C | 2.69 g/cm³ Show Material materials with Dichte of 2.69 g/cm³ | F | EN 573-3 | Profile, Rod, Flat, Tube, Plate |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Dehnung | 13.0 % Show Material materials with Dehnung of 13.0 % | F | EN 573-3, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A50 | |
15.0 % Show Material materials with Dehnung of 15.0 % | F | EN 573-3, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A100 | ||
20.0 °C | 13.0 % Show Material materials with Dehnung of 13.0 % | F | EN 573-3 | Profile, Rod, Tube | A50 | |
20.0 °C | 15.0 % Show Material materials with Dehnung of 15.0 % | F | EN 573-3 | Profile, Rod, Tube | ||
Elastizitätsmodul | 70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | F | EN 573-3, EN 1386, EN 1715-3, EN 485, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
20.0 °C | 70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | F | EN 573-3 | Profile, Rod, Flat, Tube, Plate | ||
Härte, Brinell | 20.0 °C | 47.0 [-] Show Material materials with Härte, Brinell of 47.0 [-] | F | EN 573-3 | Profile, Rod, Tube | |
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||||
Poissonzahl | 20.0 °C | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | F | EN 573-3 | Profile, Rod, Flat, Tube, Plate | |
Schubmodule | 26.3 GPa Show Material materials with Schubmodule of 26.3 GPa | F | EN 573-3, EN 1386, EN 1715-3, EN 485, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
20.0 °C | 26.3 - 27.0 GPa Show Material materials with Schubmodule of 26.3 - 27.0 GPa | F | EN 573-3 | Profile, Rod, Flat, Tube, Plate | ||
20.0 °C | 26.3 GPa Show Material materials with Schubmodule of 26.3 GPa | F | EN 573-3 | Profile, Rod, Flat, Tube, Plate | ||
Zugfestigkeit | 165.0 MPa Show Material materials with Zugfestigkeit of 165.0 MPa | F | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
170.0 MPa Show Material materials with Zugfestigkeit of 170.0 MPa | F | EN 573-3, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |||
180.0 - 250.0 MPa Show Material materials with Zugfestigkeit of 180.0 - 250.0 MPa | F | EN 573-3, EN 1715-3 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |||
20.0 °C | 165.0 MPa Show Material materials with Zugfestigkeit of 165.0 MPa | F | EN 573-3 | Flat | ||
20.0 °C | 165.0 MPa Show Material materials with Zugfestigkeit of 165.0 MPa | F | EN 573-3 | Flat | Transverse | |
20.0 °C | 170.0 MPa Show Material materials with Zugfestigkeit of 170.0 MPa | F | EN 573-3 | Profile, Rod, Tube |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | -50.0 °C | 2.21e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.21e-05 1/K | F | EN 573-3 | Profile, Rod, Flat, Tube, Plate | |
-50 °C | 2.2100000000000002e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.2100000000000002e-05 1/K | F | EN 573-3, EN 1386, EN 1715-3, EN 485, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
20 °C | 2.2100000000000002e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.2100000000000002e-05 1/K | F | EN 573-3, EN 1386, EN 1715-3, EN 485, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
20 °C | 2.38e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.38e-05 1/K | F | EN 573-3, EN 1386, EN 1715-3, EN 485, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Profile, Rod, Flat | ||
20 °C | 2.48e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.48e-05 1/K | F | EN 573-3, EN 1386, EN 1715-3, EN 485, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Profile, Rod, Flat | ||
20 °C | 2.5699999999999998e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.5699999999999998e-05 1/K | F | EN 573-3, EN 1386, EN 1715-3, EN 485, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
100 °C | 2.38e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.38e-05 1/K | F | EN 573-3, EN 1386, EN 1715-3, EN 485, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Profile, Rod, Flat | ||
100.0 °C | 2.38e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.38e-05 1/K | F | EN 573-3, EN 1386, EN 1715-3, EN 485, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Profile, Rod, Flat | ||
200 °C | 2.48e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.48e-05 1/K | F | EN 573-3, EN 1386, EN 1715-3, EN 485, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Profile, Rod, Flat | ||
200.0 °C | 2.48e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.48e-05 1/K | F | EN 573-3, EN 1386, EN 1715-3, EN 485, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Profile, Rod, Flat | ||
300 °C | 2.5699999999999998e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.5699999999999998e-05 1/K | F | EN 573-3, EN 1386, EN 1715-3, EN 485, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
300.0 °C | 2.57e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.57e-05 1/K | F | EN 573-3 | Profile, Rod, Flat, Tube, Plate | ||
Max. Betriebstemperatur | 150.0 °C Show Material materials with Max. Betriebstemperatur of 150.0 °C | Typical for Wrought 5000 Series Aluminium | ||||
Schmelzpunkt | 605.0 - 650.0 °C Show Material materials with Schmelzpunkt of 605.0 - 650.0 °C | F | EN 573-3, EN 1386, EN 1715-3, EN 485, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
607.0 - 649.0 °C Show Material materials with Schmelzpunkt of 607.0 - 649.0 °C | F | EN 573-3, EN 1386, EN 1715-3, EN 485, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |||
Spezifische Wärmekapazität | 900.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 900.0 J/(kg·K) | F | EN 573-3, EN 1386, EN 1715-3, EN 485, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
20.0 °C | 900.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 900.0 J/(kg·K) | F | EN 573-3 | Profile, Rod, Flat, Tube, Plate | ||
20.0 °C | 900.0 - 901.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 900.0 - 901.0 J/(kg·K) | F | EN 573-3 | Profile, Rod, Flat, Tube, Plate | ||
20.0 °C | 901.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 901.0 J/(kg·K) | F | EN 573-3 | Profile, Rod, Flat, Tube, Plate | ||
Wärmeleitfähigkeit | 138 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 138 W/(m·K) | F | EN 573-3, EN 1386, EN 1715-3, EN 485, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
20.0 °C | 130.0 - 150.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 130.0 - 150.0 W/(m·K) | F | EN 573-3, EN 1386, EN 1715-3, EN 485, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Profile, Rod, Flat | ||
20.0 °C | 130.0 - 138.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 130.0 - 138.0 W/(m·K) | F | EN 573-3 | Profile, Rod, Flat, Tube, Plate | ||
20.0 °C | 138.0 - 150.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 138.0 - 150.0 W/(m·K) | F | EN 573-3 | Profile, Rod, Flat, Tube, Plate | ||
20.0 °C | 138.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 138.0 W/(m·K) | F | EN 573-3 | Profile, Rod, Flat, Tube, Plate |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Elektrische Leitfähigkeit | 20000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 20000000.0 S/m | F | EN 573-3, EN 1386, EN 1715-3, EN 485, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |
20.0 °C | 19000000.0 - 21000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 19000000.0 - 21000000.0 S/m | F | EN 573-3, EN 1386, EN 1715-3, EN 485, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Profile, Rod, Flat | |
spezifischer Widerstand | 4.76e-08 - 5.26e-08 Ω·m Show Material materials with spezifischer Widerstand of 4.76e-08 - 5.26e-08 Ω·m | F | EN 573-3, EN 1386, EN 1715-3, EN 485, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |
5e-08 Ω·m Show Material materials with spezifischer Widerstand of 5e-08 Ω·m | F | EN 573-3, EN 1386, EN 1715-3, EN 485, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
20.0 °C | 4.7e-08 - 4.95e-08 Ω·m Show Material materials with spezifischer Widerstand of 4.7e-08 - 4.95e-08 Ω·m | F | EN 573-3 | Profile, Rod, Flat, Tube, Plate | |
20.0 °C | 4.7e-08 - 5.2e-08 Ω·m Show Material materials with spezifischer Widerstand of 4.7e-08 - 5.2e-08 Ω·m | F | EN 573-3 | Profile, Rod, Flat, Tube, Plate | |
20.0 °C | 4.95e-08 Ω·m Show Material materials with spezifischer Widerstand of 4.95e-08 Ω·m | F | EN 573-3 | Profile, Rod, Flat, Tube, Plate | |
20.0 °C | 4.95e-08 - 5.2e-08 Ω·m Show Material materials with spezifischer Widerstand of 4.95e-08 - 5.2e-08 Ω·m | F | EN 573-3 | Profile, Rod, Flat, Tube, Plate |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chrom | 0.15 - 0.35 % Show Material materials with Chrom of 0.15 - 0.35 % | F | EN 573-3, EN 1386, EN 1715-3, EN 485, EN 755 | Profile, Rod, Flat, Tube, Plate, Strip, Sheet, Foil, Wire, Bar |
Eisen | 0.4 % Show Material materials with Eisen of 0.4 % | F | EN 573-3 | Profile, Rod, Flat, Tube, Plate |
0.40 % Show Material materials with Eisen of 0.40 % | F | EN 573-3, EN 1386, EN 1715-3, EN 485, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |
Kupfer | 0.1 % Show Material materials with Kupfer of 0.1 % | F | EN 573-3, EN 1386, EN 1715-3, EN 485, EN 755 | Profile, Rod, Flat, Tube, Plate, Strip, Sheet, Foil, Wire, Bar |
Magnesium | 2.2 - 2.8 % Show Material materials with Magnesium of 2.2 - 2.8 % | F | EN 573-3, EN 1386, EN 1715-3, EN 485, EN 755 | Profile, Rod, Flat, Tube, Plate, Strip, Sheet, Foil, Wire, Bar |
Mangan | 0.1 % Show Material materials with Mangan of 0.1 % | F | EN 573-3, EN 1386, EN 1715-3, EN 485, EN 755 | Profile, Rod, Flat, Tube, Plate, Strip, Sheet, Foil, Wire, Bar |
Silizium | 0.25 % Show Material materials with Silizium of 0.25 % | F | EN 573-3, EN 1386, EN 1715-3, EN 485, EN 755 | Profile, Rod, Flat, Tube, Plate, Strip, Sheet, Foil, Wire, Bar |
Zink | 0.1 % Show Material materials with Zink of 0.1 % | F | EN 573-3, EN 1386, EN 1715-3, EN 485, EN 755 | Profile, Rod, Flat, Tube, Plate, Strip, Sheet, Foil, Wire, Bar |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: good, Protective: very good | |
Corrosion properties | Seawater: very good to good, weathering: good | |
Workability | Bending / Spinning (cold): very good / acceptable, Impact extrusion (cold): acceptable, Deep drawing / upsetting (Condition) good (O) / good (H12) |