Allgemein
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 2.68 g/cm³ Show Material materials with Dichte of 2.68 g/cm³ | H111 | EN 573-3, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |
20.0 °C | 2.68 g/cm³ Show Material materials with Dichte of 2.68 g/cm³ | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541, EN 573-3 | Sheet, Rod, Flat, Tube | |
20.0 °C | 2.68 - 2.69 g/cm³ Show Material materials with Dichte of 2.68 - 2.69 g/cm³ | H111 | EN 573-3 | Rod, Flat, Tube | |
20.0 °C | 2.69 g/cm³ Show Material materials with Dichte of 2.69 g/cm³ | H111 | EN 573-3 | Rod, Flat, Tube |
Abmessung
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Biegewinkel 180° | 0 °/t Show Material materials with Biegewinkel 180° of 0 °/t | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet | ||
0.5 °/t Show Material materials with Biegewinkel 180° of 0.5 °/t | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |||
Biegewinkel 90° | 0 °/t Show Material materials with Biegewinkel 90° of 0 °/t | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet | ||
0.5 °/t Show Material materials with Biegewinkel 90° of 0.5 °/t | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |||
1.0 °/t Show Material materials with Biegewinkel 90° of 1.0 °/t | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |||
2.0 °/t Show Material materials with Biegewinkel 90° of 2.0 °/t | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |||
Dehnung | 12.0 % Show Material materials with Dehnung of 12.0 % | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A50 | |
12 % Show Material materials with Dehnung of 12 % | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet | A50 | ||
14.0 % Show Material materials with Dehnung of 14.0 % | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A50 | ||
15.0 % Show Material materials with Dehnung of 15.0 % | H111 | EN 573-3, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A50 | ||
16.0 % Show Material materials with Dehnung of 16.0 % | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A50 | ||
17.0 % Show Material materials with Dehnung of 17.0 % | H111 | EN 573-3, EN 754 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A50 | ||
17.0 % Show Material materials with Dehnung of 17.0 % | H111 | EN 573-3, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A100 | ||
18.0 % Show Material materials with Dehnung of 18.0 % | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A50 | ||
18.0 % Show Material materials with Dehnung of 18.0 % | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A100 | ||
19.0 % Show Material materials with Dehnung of 19.0 % | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A50 | ||
20.0 % Show Material materials with Dehnung of 20.0 % | H111 | EN 573-3, EN 754 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A100 | ||
20.0 °C | 12.0 % Show Material materials with Dehnung of 12.0 % | H111 | EN 573-3 | Flat | A50 | |
20.0 °C | 12.0 % Show Material materials with Dehnung of 12.0 % | H111 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 14.0 % Show Material materials with Dehnung of 14.0 % | H111 | EN 573-3 | Flat | A50 | |
20.0 °C | 14.0 % Show Material materials with Dehnung of 14.0 % | H111 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 15.0 % Show Material materials with Dehnung of 15.0 % | H111 | EN 573-3 | Rod, Tube | A50 | |
20.0 °C | 16.0 % Show Material materials with Dehnung of 16.0 % | H111 | EN 573-3 | Flat | A50 | |
20.0 °C | 16.0 % Show Material materials with Dehnung of 16.0 % | H111 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 17.0 % Show Material materials with Dehnung of 17.0 % | H111 | EN 573-3 | Rod, Tube | A50 | |
20.0 °C | 17.0 % Show Material materials with Dehnung of 17.0 % | H111 | EN 573-3 | Rod, Tube | ||
20.0 °C | 18.0 % Show Material materials with Dehnung of 18.0 % | H111 | EN 573-3 | Flat | A50 | |
20.0 °C | 18.0 % Show Material materials with Dehnung of 18.0 % | H111 | EN 573-3 | Flat | ||
20.0 °C | 18.0 % Show Material materials with Dehnung of 18.0 % | H111 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 18.0 % Show Material materials with Dehnung of 18.0 % | H111 | EN 573-3 | Flat | Transverse | |
20.0 °C | 19.0 % Show Material materials with Dehnung of 19.0 % | H111 | EN 573-3 | Flat | A50 | |
20.0 °C | 19.0 % Show Material materials with Dehnung of 19.0 % | H111 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 20.0 % Show Material materials with Dehnung of 20.0 % | H111 | EN 573-3 | Rod, Tube | ||
Elastizitätsmodul | 70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | H111 | EN 573-3, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
20.0 °C | 70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541, EN 573-3 | Sheet, Rod, Flat, Tube | ||
Härte, Brinell | 46.0 [-] Show Material materials with Härte, Brinell of 46.0 [-] | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
47.0 [-] Show Material materials with Härte, Brinell of 47.0 [-] | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |||
20.0 °C | 45.0 [-] Show Material materials with Härte, Brinell of 45.0 [-] | H111 | EN 573-3 | Rod, Tube | ||
20.0 °C | 46.0 - 47.0 [-] Show Material materials with Härte, Brinell of 46.0 - 47.0 [-] | H111 | EN 573-3 | Flat | ||
20.0 °C | 46.0 [-] Show Material materials with Härte, Brinell of 46.0 [-] | H111 | EN 573-3 | Flat | ||
20.0 °C | 47.0 [-] Show Material materials with Härte, Brinell of 47.0 [-] | H111 | EN 573-3 | Rod, Tube, Flat | ||
Härte, HBW | 47 [-] Show Material materials with Härte, HBW of 47 [-] | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||||
Poissonzahl | 20.0 °C | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | H111 | EN 573-3 | Rod, Flat, Tube | |
Schubmodule | 26.3 GPa Show Material materials with Schubmodule of 26.3 GPa | H111 | EN 573-3, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
26.5 GPa Show Material materials with Schubmodule of 26.5 GPa | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet | |||
20.0 °C | 26.3 - 27.0 GPa Show Material materials with Schubmodule of 26.3 - 27.0 GPa | H111 | EN 573-3 | Rod, Flat, Tube | ||
20.0 °C | 26.3 GPa Show Material materials with Schubmodule of 26.3 GPa | H111 | EN 573-3 | Rod, Flat, Tube | ||
Streckgrenze | 65.0 MPa Show Material materials with Streckgrenze of 65.0 MPa | H111 | EN 573-3, EN 485, EN 754 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | RP02 | |
65 MPa Show Material materials with Streckgrenze of 65 MPa | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet | |||
70.0 MPa Show Material materials with Streckgrenze of 70.0 MPa | H111 | EN 573-3, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | RP02 | ||
20.0 °C | 65.0 MPa Show Material materials with Streckgrenze of 65.0 MPa | H111 | EN 573-3 | Rod, Tube, Flat | RP02 | |
20.0 °C | 65.0 MPa Show Material materials with Streckgrenze of 65.0 MPa | H111 | EN 573-3 | Flat | RP02 Transverse | |
20.0 °C | 70.0 MPa Show Material materials with Streckgrenze of 70.0 MPa | H111 | EN 573-3 | Rod, Tube | RP02 | |
Zugfestigkeit | 20.0 °C | 165.0 - 215.0 MPa Show Material materials with Zugfestigkeit of 165.0 - 215.0 MPa | H111 | EN 573-3, EN 485 | Flat, Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |
20.0 °C | 165.0 - 215.0 MPa Show Material materials with Zugfestigkeit of 165.0 - 215.0 MPa | H111 | EN 573-3 | Flat | Transverse | |
20.0 °C | 170.0 MPa Show Material materials with Zugfestigkeit of 170.0 MPa | H111 | EN 573-3 | Rod | ||
20.0 °C | 170.0 - 230.0 MPa Show Material materials with Zugfestigkeit of 170.0 - 230.0 MPa | H111 | EN 573-3, EN 754, EN 755 | Rod, Tube, Strip, Sheet, Plate, Foil, Wire, Bar | ||
20.0 °C | 170.0 - 215.0 MPa Show Material materials with Zugfestigkeit of 170.0 - 215.0 MPa | H111 | EN 573-3, EN 485, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Flat, Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
20.0 °C | 170.0 - 215.0 MPa Show Material materials with Zugfestigkeit of 170.0 - 215.0 MPa | H111 | EN 573-3 | Flat | Transverse |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | -50.0 °C | 2.21e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.21e-05 1/K | H111 | EN 573-3 | Rod, Flat, Tube | |
-50 °C | 2.2100000000000002e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.2100000000000002e-05 1/K | H111 | EN 573-3, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
20 °C | 2.2100000000000002e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.2100000000000002e-05 1/K | H111 | EN 573-3, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
20 °C | 2.38e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.38e-05 1/K | H111 | EN 573-3, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Rod, Flat | ||
20 °C | 2.48e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.48e-05 1/K | H111 | EN 573-3, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Rod, Flat | ||
20 °C | 2.5699999999999998e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.5699999999999998e-05 1/K | H111 | EN 573-3, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
100 °C | 2.38e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.38e-05 1/K | H111 | EN 573-3, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Rod, Flat | ||
100.0 °C | 2.38e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.38e-05 1/K | H111 | EN 573-3, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Rod, Flat | ||
100 °C | 0.000024 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 0.000024 1/K | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet | 20-100°C | |
200 °C | 2.48e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.48e-05 1/K | H111 | EN 573-3, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Rod, Flat | ||
200.0 °C | 2.48e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.48e-05 1/K | H111 | EN 573-3, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Rod, Flat | ||
300 °C | 2.5699999999999998e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.5699999999999998e-05 1/K | H111 | EN 573-3, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
300.0 °C | 2.57e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.57e-05 1/K | H111 | EN 573-3 | Rod, Flat, Tube | ||
Max. Betriebstemperatur | 150.0 °C Show Material materials with Max. Betriebstemperatur of 150.0 °C | Typical for Wrought 5000 Series Aluminium | ||||
Schmelzpunkt | 605.0 - 650.0 °C Show Material materials with Schmelzpunkt of 605.0 - 650.0 °C | H111 | EN 573-3, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
607.0 - 649.0 °C Show Material materials with Schmelzpunkt of 607.0 - 649.0 °C | H111 | EN 573-3, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |||
Spezifische Wärmekapazität | 900.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 900.0 J/(kg·K) | H111 | EN 573-3, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
20.0 °C | 900.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 900.0 J/(kg·K) | H111 | EN 573-3 | Rod, Flat, Tube | ||
20.0 °C | 900.0 - 901.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 900.0 - 901.0 J/(kg·K) | H111 | EN 573-3 | Rod, Flat, Tube | ||
20.0 °C | 901.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 901.0 J/(kg·K) | H111 | EN 573-3 | Rod, Flat, Tube | ||
Wärmeleitfähigkeit | 138 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 138 W/(m·K) | H111 | EN 573-3, EN 485, EN 13195, EN 754, EN 755, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
20.0 °C | 130.0 - 150.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 130.0 - 150.0 W/(m·K) | H111 | EN 573-3, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Rod, Flat | ||
20.0 °C | 130.0 - 138.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 130.0 - 138.0 W/(m·K) | H111 | EN 573-3 | Rod, Flat, Tube | ||
20.0 °C | 138.0 - 150.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 138.0 - 150.0 W/(m·K) | H111 | EN 573-3 | Rod, Flat, Tube | ||
20.0 °C | 138.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 138.0 W/(m·K) | H111 | EN 573-3 | Rod, Flat, Tube |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Elektrische Leitfähigkeit | 20000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 20000000.0 S/m | H111 | EN 573-3, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |
20.0 °C | 19000000.0 - 21000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 19000000.0 - 21000000.0 S/m | H111 | EN 573-3, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Rod, Flat | |
spezifischer Widerstand | 4.76e-08 - 5.26e-08 Ω·m Show Material materials with spezifischer Widerstand of 4.76e-08 - 5.26e-08 Ω·m | H111 | EN 573-3, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |
4.9e-08 Ω·m Show Material materials with spezifischer Widerstand of 4.9e-08 Ω·m | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet | ||
5e-08 Ω·m Show Material materials with spezifischer Widerstand of 5e-08 Ω·m | H111 | EN 573-3, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
20.0 °C | 4.7e-08 - 4.95e-08 Ω·m Show Material materials with spezifischer Widerstand of 4.7e-08 - 4.95e-08 Ω·m | H111 | EN 573-3 | Rod, Flat, Tube | |
20.0 °C | 4.7e-08 - 5.2e-08 Ω·m Show Material materials with spezifischer Widerstand of 4.7e-08 - 5.2e-08 Ω·m | H111 | EN 573-3 | Rod, Flat, Tube | |
20.0 °C | 4.95e-08 Ω·m Show Material materials with spezifischer Widerstand of 4.95e-08 Ω·m | H111 | EN 573-3 | Rod, Flat, Tube | |
20.0 °C | 4.95e-08 - 5.2e-08 Ω·m Show Material materials with spezifischer Widerstand of 4.95e-08 - 5.2e-08 Ω·m | H111 | EN 573-3 | Rod, Flat, Tube |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Andere | 0.15 % Show Material materials with Andere of 0.15 % | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet |
Chrom | 0.15 - 0.35 % Show Material materials with Chrom of 0.15 - 0.35 % | H111 | EN 573-3, EN 485, EN 13195, EN 754, EN 755, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Rod, Flat, Tube, Strip, Sheet, Plate, Foil, Wire, Bar |
Eisen | 0.4 % Show Material materials with Eisen of 0.4 % | H111 | EN 573-3 | Rod, Flat, Tube |
0.40 % Show Material materials with Eisen of 0.40 % | H111 | EN 573-3, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |
0.4 % Show Material materials with Eisen of 0.4 % | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet | |
Kupfer | 0.1 % Show Material materials with Kupfer of 0.1 % | H111 | EN 573-3, EN 485, EN 13195, EN 754, EN 755 | Rod, Flat, Tube, Strip, Sheet, Plate, Foil, Wire, Bar |
0.1 % Show Material materials with Kupfer of 0.1 % | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet | |
Magnesium | 2.2 - 2.8 % Show Material materials with Magnesium of 2.2 - 2.8 % | H111 | EN 573-3, EN 485, EN 13195, EN 754, EN 755, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Rod, Flat, Tube, Strip, Sheet, Plate, Foil, Wire, Bar |
Mangan | 0.1 % Show Material materials with Mangan of 0.1 % | H111 | EN 573-3, EN 485, EN 13195, EN 754, EN 755 | Rod, Flat, Tube, Strip, Sheet, Plate, Foil, Wire, Bar |
0.1 % Show Material materials with Mangan of 0.1 % | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet | |
Silizium | 0.25 % Show Material materials with Silizium of 0.25 % | H111 | EN 573-3, EN 485, EN 13195, EN 754, EN 755 | Rod, Flat, Tube, Strip, Sheet, Plate, Foil, Wire, Bar |
0.25 % Show Material materials with Silizium of 0.25 % | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet | |
Zink | 0.1 % Show Material materials with Zink of 0.1 % | H111 | EN 573-3, EN 485, EN 13195, EN 754, EN 755 | Rod, Flat, Tube, Strip, Sheet, Plate, Foil, Wire, Bar |
0.1 % Show Material materials with Zink of 0.1 % | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: good, Protective: very good | |
Application areas | Facades: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Doors: Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Interiors and ceilings: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Furniture, Plinths, Blinds: Single sheet, Intermediate transformation/interior use; Anodizing quality; Electronic devices: Housing devices; Closures: Easy open; Food can: Body, Lids; Components: Heat shields, Access hatches, Spoilers, General trasportation | |
Corrosion properties | Seawater: very good to good, weathering: good | |
Welding | Very Good | |
Workability | Bending / Spinning (cold): very good / acceptable, Impact extrusion (cold): acceptable, Deep drawing / upsetting (Condition) good (O) / good (H12) |