Allgemein
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 2.68 g/cm³ Show Material materials with Dichte of 2.68 g/cm³ | H46 | EN 573-3, EN 1396, EN 541 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |
20.0 °C | 2.68 g/cm³ Show Material materials with Dichte of 2.68 g/cm³ | H46 | EN 573-3 | Sheet, Strip | |
20.0 °C | 2.68 - 2.69 g/cm³ Show Material materials with Dichte of 2.68 - 2.69 g/cm³ | H46 | EN 573-3 | Sheet, Strip | |
20.0 °C | 2.69 g/cm³ Show Material materials with Dichte of 2.69 g/cm³ | H46 | EN 573-3 | Sheet, Strip |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 125.0 MPa Show Material materials with Bending Fatigue Strength of 125.0 MPa | H46 | EN 573-3, EN 1396, EN 541 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
Elastizitätsmodul | 70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | H46 | EN 573-3, EN 1396, EN 541 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
20.0 °C | 70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | H46 | EN 573-3 | Sheet, Strip | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||||
Poissonzahl | 20.0 °C | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | H46 | EN 573-3 | Sheet, Strip | |
Schubmodule | 26.3 GPa Show Material materials with Schubmodule of 26.3 GPa | H46 | EN 573-3, EN 1396, EN 541 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
20.0 °C | 26.3 - 27.0 GPa Show Material materials with Schubmodule of 26.3 - 27.0 GPa | H46 | EN 573-3 | Sheet, Strip | ||
20.0 °C | 26.3 GPa Show Material materials with Schubmodule of 26.3 GPa | H46 | EN 573-3 | Sheet, Strip | ||
Zugfestigkeit | 240.0 - 280.0 MPa Show Material materials with Zugfestigkeit of 240.0 - 280.0 MPa | H46 | EN 573-3, EN 541 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
20.0 °C | 250.0 - 300.0 MPa Show Material materials with Zugfestigkeit of 250.0 - 300.0 MPa | H46 | EN 573-3 | Sheet, Strip | Transverse | |
20.0 °C | 250.0 - 300.0 MPa Show Material materials with Zugfestigkeit of 250.0 - 300.0 MPa | H46 | EN 573-3, EN 1396 | Sheet, Strip, Plate, Foil, Wire, Tube, Bar | ||
20.0 °C | 260.0 - 300.0 MPa Show Material materials with Zugfestigkeit of 260.0 - 300.0 MPa | H46 | EN 573-3, EN 541 | Sheet, Strip, Plate, Foil, Wire, Tube, Bar |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | -50.0 °C | 2.21e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.21e-05 1/K | H46 | EN 573-3 | Sheet, Strip | |
-50 °C | 2.2100000000000002e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.2100000000000002e-05 1/K | H46 | EN 573-3, EN 1396, EN 541 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
20 °C | 2.2100000000000002e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.2100000000000002e-05 1/K | H46 | EN 573-3, EN 1396, EN 541 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
20 °C | 2.38e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.38e-05 1/K | H46 | EN 573-3, EN 1396, EN 541 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
20 °C | 2.48e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.48e-05 1/K | H46 | EN 573-3, EN 1396, EN 541 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
20 °C | 2.5699999999999998e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.5699999999999998e-05 1/K | H46 | EN 573-3, EN 1396, EN 541 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
100 °C | 2.38e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.38e-05 1/K | H46 | EN 573-3, EN 1396, EN 541 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
100.0 °C | 2.38e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.38e-05 1/K | H46 | EN 573-3, EN 1396, EN 541 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
200 °C | 2.48e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.48e-05 1/K | H46 | EN 573-3, EN 1396, EN 541 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
200.0 °C | 2.48e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.48e-05 1/K | H46 | EN 573-3, EN 1396, EN 541 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
300 °C | 2.5699999999999998e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.5699999999999998e-05 1/K | H46 | EN 573-3, EN 1396, EN 541 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
300.0 °C | 2.57e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.57e-05 1/K | H46 | EN 573-3 | Sheet, Strip | ||
Max. Betriebstemperatur | 150.0 °C Show Material materials with Max. Betriebstemperatur of 150.0 °C | Typical for Wrought 5000 Series Aluminium | ||||
Schmelzpunkt | 605.0 - 650.0 °C Show Material materials with Schmelzpunkt of 605.0 - 650.0 °C | H46 | EN 573-3, EN 1396, EN 541 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
607.0 - 649.0 °C Show Material materials with Schmelzpunkt of 607.0 - 649.0 °C | H46 | EN 573-3, EN 1396, EN 541 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |||
Spezifische Wärmekapazität | 900.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 900.0 J/(kg·K) | H46 | EN 573-3, EN 1396, EN 541 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
20.0 °C | 900.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 900.0 J/(kg·K) | H46 | EN 573-3 | Sheet, Strip | ||
20.0 °C | 900.0 - 901.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 900.0 - 901.0 J/(kg·K) | H46 | EN 573-3 | Sheet, Strip | ||
20.0 °C | 901.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 901.0 J/(kg·K) | H46 | EN 573-3 | Sheet, Strip | ||
Wärmeleitfähigkeit | 138 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 138 W/(m·K) | H46 | EN 573-3, EN 1396, EN 541 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
20.0 °C | 130.0 - 150.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 130.0 - 150.0 W/(m·K) | H46 | EN 573-3, EN 1396, EN 541 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
20.0 °C | 130.0 - 138.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 130.0 - 138.0 W/(m·K) | H46 | EN 573-3 | Sheet, Strip | ||
20.0 °C | 138.0 - 150.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 138.0 - 150.0 W/(m·K) | H46 | EN 573-3 | Sheet, Strip | ||
20.0 °C | 138.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 138.0 W/(m·K) | H46 | EN 573-3 | Sheet, Strip |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Elektrische Leitfähigkeit | 20000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 20000000.0 S/m | H46 | EN 573-3, EN 1396, EN 541 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |
20.0 °C | 19000000.0 - 21000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 19000000.0 - 21000000.0 S/m | H46 | EN 573-3, EN 1396, EN 541 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |
spezifischer Widerstand | 4.76e-08 - 5.26e-08 Ω·m Show Material materials with spezifischer Widerstand of 4.76e-08 - 5.26e-08 Ω·m | H46 | EN 573-3, EN 1396, EN 541 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |
5e-08 Ω·m Show Material materials with spezifischer Widerstand of 5e-08 Ω·m | H46 | EN 573-3, EN 1396, EN 541 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
20.0 °C | 4.7e-08 - 4.95e-08 Ω·m Show Material materials with spezifischer Widerstand of 4.7e-08 - 4.95e-08 Ω·m | H46 | EN 573-3 | Sheet, Strip | |
20.0 °C | 4.7e-08 - 5.2e-08 Ω·m Show Material materials with spezifischer Widerstand of 4.7e-08 - 5.2e-08 Ω·m | H46 | EN 573-3 | Sheet, Strip | |
20.0 °C | 4.95e-08 Ω·m Show Material materials with spezifischer Widerstand of 4.95e-08 Ω·m | H46 | EN 573-3 | Sheet, Strip | |
20.0 °C | 4.95e-08 - 5.2e-08 Ω·m Show Material materials with spezifischer Widerstand of 4.95e-08 - 5.2e-08 Ω·m | H46 | EN 573-3 | Sheet, Strip |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chrom | 0.15 - 0.35 % Show Material materials with Chrom of 0.15 - 0.35 % | H46 | EN 573-3, EN 1396, EN 541 | Sheet, Strip, Plate, Foil, Wire, Tube, Bar |
Eisen | 0.4 % Show Material materials with Eisen of 0.4 % | H46 | EN 573-3 | Sheet, Strip |
0.40 % Show Material materials with Eisen of 0.40 % | H46 | EN 573-3, EN 1396, EN 541 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |
Kupfer | 0.1 % Show Material materials with Kupfer of 0.1 % | H46 | EN 573-3, EN 1396, EN 541 | Sheet, Strip, Plate, Foil, Wire, Tube, Bar |
Magnesium | 2.2 - 2.8 % Show Material materials with Magnesium of 2.2 - 2.8 % | H46 | EN 573-3, EN 1396, EN 541 | Sheet, Strip, Plate, Foil, Wire, Tube, Bar |
Mangan | 0.1 % Show Material materials with Mangan of 0.1 % | H46 | EN 573-3, EN 1396, EN 541 | Sheet, Strip, Plate, Foil, Wire, Tube, Bar |
Silizium | 0.25 % Show Material materials with Silizium of 0.25 % | H46 | EN 573-3, EN 1396, EN 541 | Sheet, Strip, Plate, Foil, Wire, Tube, Bar |
Zink | 0.1 % Show Material materials with Zink of 0.1 % | H46 | EN 573-3, EN 1396, EN 541 | Sheet, Strip, Plate, Foil, Wire, Tube, Bar |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: good, Protective: very good | |
Corrosion properties | Seawater: very good to good, weathering: good | |
Workability | Bending / Spinning (cold): very good / acceptable, Impact extrusion (cold): acceptable, Deep drawing / upsetting (Condition) good (O) / good (H12) |