Allgemein
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Dichte | 2.7 g/cmÂł Show Material materials with Dichte of 2.7 g/cmÂł | F | EN 573-3, EN 1715-3, EN 570 | Strip, Sheet, Plate |
Mechanisch
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
ElastizitÀtsmodul | 70.0 GPa Show Material materials with ElastizitÀtsmodul of 70.0 GPa | F | EN 573-3, EN 1715-3, EN 570 | Strip, Sheet, Plate | |
HĂ€rte, Brinell | 18.0 [-] Show Material materials with HĂ€rte, Brinell of 18.0 [-] | F | EN 573-3, EN 570 | Strip, Sheet, Plate | |
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·âm Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·âm | Typical for Wrought 1000 Series Aluminium | |||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 1000 Series Aluminium | |||
Schubmodule | 25.9 GPa Show Material materials with Schubmodule of 25.9 GPa | Typical for Wrought 1000 Series Aluminium | |||
Zugfestigkeit | 75.0 - 85.0 MPa Show Material materials with Zugfestigkeit of 75.0 - 85.0 MPa | F | EN 573-3, EN 1715-3 | Strip, Sheet, Plate |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | -50 °C | 2.18e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.18e-05 1/K | F | EN 573-3, EN 1715-3, EN 570 | Strip, Sheet, Plate |
20 °C | 2.18e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.18e-05 1/K | F | EN 573-3, EN 1715-3, EN 570 | Strip, Sheet, Plate | |
20 °C | 2.35e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.35e-05 1/K | F | EN 573-3, EN 1715-3, EN 570 | Strip, Sheet, Plate | |
20 °C | 2.45e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.45e-05 1/K | F | EN 573-3, EN 1715-3, EN 570 | Strip, Sheet, Plate | |
20 °C | 2.55e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.55e-05 1/K | F | EN 573-3, EN 1715-3, EN 570 | Strip, Sheet, Plate | |
100 °C | 2.35e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.35e-05 1/K | F | EN 573-3, EN 1715-3, EN 570 | Strip, Sheet, Plate | |
200 °C | 2.45e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.45e-05 1/K | F | EN 573-3, EN 1715-3, EN 570 | Strip, Sheet, Plate | |
300 °C | 2.55e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.55e-05 1/K | F | EN 573-3, EN 1715-3, EN 570 | Strip, Sheet, Plate | |
Schmelzpunkt | 660.0 °C Show Material materials with Schmelzpunkt of 660.0 °C | F | EN 573-3, EN 1715-3, EN 570 | Strip, Sheet, Plate | |
Spezifische WÀrmekapazitÀt | 900.0 J/(kg·K) Show Material materials with Spezifische WÀrmekapazitÀt of 900.0 J/(kg·K) | F | EN 573-3, EN 1715-3, EN 570 | Strip, Sheet, Plate | |
WÀrmeleitfÀhigkeit | 232 W/(m·K) Show Material materials with WÀrmeleitfÀhigkeit of 232 W/(m·K) | F | EN 573-3, EN 1715-3, EN 570 | Strip, Sheet, Plate |
Elektrisch
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Elektrische LeitfÀhigkeit | 37500000.0 - 37700000.0 S/m Show Material materials with Elektrische LeitfÀhigkeit of 37500000.0 - 37700000.0 S/m | F | EN 573-3, EN 1715-3, EN 570 | Strip, Sheet, Plate |
spezifischer Widerstand | 2.65e-08 - 2.67e-08 Ω·m Show Material materials with spezifischer Widerstand of 2.65e-08 - 2.67e-08 Ω·m | F | EN 573-3, EN 1715-3, EN 570 | Strip, Sheet, Plate |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminium | 99.98 % Show Material materials with Aluminium of 99.98 % | F | EN 573-3, EN 1715-3, EN 570 | Strip, Sheet, Plate |
Eisen | 0.006 % Show Material materials with Eisen of 0.006 % | F | EN 573-3, EN 1715-3, EN 570 | Strip, Sheet, Plate |
Kupfer | 0.003 % Show Material materials with Kupfer of 0.003 % | F | EN 573-3, EN 1715-3, EN 570 | Strip, Sheet, Plate |
Silizium | 0.01 % Show Material materials with Silizium of 0.01 % | F | EN 573-3, EN 1715-3, EN 570 | Strip, Sheet, Plate |
Titan | 0.003 % Show Material materials with Titan of 0.003 % | F | EN 573-3, EN 1715-3, EN 570 | Strip, Sheet, Plate |
Zink | 0.015 % Show Material materials with Zink of 0.015 % | F | EN 573-3, EN 1715-3, EN 570 | Strip, Sheet, Plate |
Technological properties
Property | ||
---|---|---|
Brazing | hard brazing (with flux/ without flux): very good / very good, friction soldering: very good, soft brazing with flux: very good, general: very good | |
Corrosion properties | Seawater: acceptable, weathering: good | |
Workability | Bending / Spinning (cold): very good |