Allgemein
Property | Value | Condition | Related Standards |
---|---|---|---|
Dichte | 2.79 g/cm³ Show Material materials with Dichte of 2.79 g/cm³ | H13 | AA Standards, ASTM B316 |
Mechanisch
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Elastizitätsmodul | 73.0 GPa Show Material materials with Elastizitätsmodul of 73.0 GPa | H13 | AA Standards, ASTM B316 | |
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 2000 Series Aluminium | ||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 2000 Series Aluminium | ||
Schubmodule | 26.0 - 27.5 GPa Show Material materials with Schubmodule of 26.0 - 27.5 GPa | Typical for Wrought 2000 Series Aluminium | ||
Zugfestigkeit | 205.0 - 275.0 MPa Show Material materials with Zugfestigkeit of 205.0 - 275.0 MPa | H13 | AA Standards, ASTM B316 |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Comment |
---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 20 °C | 2.36e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.36e-05 1/K | H13 | AA Standards, ASTM B316 | |
100 °C | 2.36e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.36e-05 1/K | H13 | AA Standards, ASTM B316 | ||
Schmelzpunkt | 510.0 - 640.0 °C Show Material materials with Schmelzpunkt of 510.0 - 640.0 °C | H13 | AA Standards, ASTM B316 | ||
Spezifische Wärmekapazität | 816.0 - 963.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 816.0 - 963.0 J/(kg·K) | Typical for Wrought 2000 Series Aluminium | |||
Wärmeleitfähigkeit | 134.0 - 193.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 134.0 - 193.0 W/(m·K) | H13 | AA Standards, ASTM B316 |
Elektrisch
Property | Value | Condition | Related Standards |
---|---|---|---|
Elektrische Leitfähigkeit | 20000000.0 - 29000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 20000000.0 - 29000000.0 S/m | H13 | AA Standards, ASTM B316 |
spezifischer Widerstand | 3.45e-08 - 5e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.45e-08 - 5e-08 Ω·m | H13 | AA Standards, ASTM B316 |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Chrom | 0.1 % Show Material materials with Chrom of 0.1 % | H13 | AA Standards, ASTM B316 |
Eisen | 0.70 % Show Material materials with Eisen of 0.70 % | H13 | AA Standards, ASTM B316 |
Kupfer | 3.5 - 4.5 % Show Material materials with Kupfer of 3.5 - 4.5 % | H13 | AA Standards, ASTM B316 |
Magnesium | 0.4 - 0.8 % Show Material materials with Magnesium of 0.4 - 0.8 % | H13 | AA Standards, ASTM B316 |
Mangan | 0.4 - 1.0 % Show Material materials with Mangan of 0.4 - 1.0 % | H13 | AA Standards, ASTM B316 |
Silizium | 0.2 - 0.8 % Show Material materials with Silizium of 0.2 - 0.8 % | H13 | AA Standards, ASTM B316 |
Titan | 0.15 % Show Material materials with Titan of 0.15 % | H13 | AA Standards, ASTM B316 |
Zink | 0.25 % Show Material materials with Zink of 0.25 % | H13 | AA Standards, ASTM B316 |
Technological properties
Property | ||
---|---|---|
Brazing | general: no brazing is known or developed | |
Corrosion properties | Stress corrosion cracking: Operational damage in areas with tensile stresses transverse to the grain structure, limited damage to laboratory samples, general: sufficient, in principle it should be protected | |
General machinability | General: good to acceptable | |
Workability | general (condition): poor(T4, T451) |