Allgemein
Property | Value | Condition | Related Standards |
---|---|---|---|
Dichte | 2.82 g/cm³ Show Material materials with Dichte of 2.82 g/cm³ | T61 | AA Standards, ASTM B247 |
Mechanisch
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Bending Fatigue Strength | 115.0 MPa Show Material materials with Bending Fatigue Strength of 115.0 MPa | T61 | AA Standards | |
Elastizitätsmodul | 74.0 GPa Show Material materials with Elastizitätsmodul of 74.0 GPa | T61 | AA Standards, ASTM B247 | |
Härte, Brinell | 120.0 [-] Show Material materials with Härte, Brinell of 120.0 [-] | T61 | AA Standards | |
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 2000 Series Aluminium | ||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 2000 Series Aluminium | ||
Schubmodule | 26.0 - 27.5 GPa Show Material materials with Schubmodule of 26.0 - 27.5 GPa | Typical for Wrought 2000 Series Aluminium | ||
Zugfestigkeit | 380.0 MPa Show Material materials with Zugfestigkeit of 380.0 MPa | T61 | AA Standards, ASTM B247 | |
420.0 MPa Show Material materials with Zugfestigkeit of 420.0 MPa | T61 | AA Standards |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Comment |
---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 20 °C | 2.23e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.23e-05 1/K | T61 | AA Standards, ASTM B247 | |
100 °C | 2.23e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.23e-05 1/K | T61 | AA Standards, ASTM B247 | ||
Schmelzpunkt | 505.0 - 640.0 °C Show Material materials with Schmelzpunkt of 505.0 - 640.0 °C | T61 | AA Standards, ASTM B247 | ||
Spezifische Wärmekapazität | 816.0 - 963.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 816.0 - 963.0 J/(kg·K) | Typical for Wrought 2000 Series Aluminium | |||
Wärmeleitfähigkeit | 155 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 155 W/(m·K) | T61 | AA Standards, ASTM B247 |
Elektrisch
Property | Value | Condition | Related Standards |
---|---|---|---|
Elektrische Leitfähigkeit | 23000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 23000000.0 S/m | T61 | AA Standards, ASTM B247 |
spezifischer Widerstand | 4.35e-08 Ω·m Show Material materials with spezifischer Widerstand of 4.35e-08 Ω·m | T61 | AA Standards, ASTM B247 |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Chrom | 0.1 % Show Material materials with Chrom of 0.1 % | T61 | AA Standards, ASTM B247 |
Eisen | 1.00 % Show Material materials with Eisen of 1.00 % | T61 | AA Standards, ASTM B247 |
Kupfer | 3.5 - 4.5 % Show Material materials with Kupfer of 3.5 - 4.5 % | T61 | AA Standards, ASTM B247 |
Magnesium | 0.45 - 0.9 % Show Material materials with Magnesium of 0.45 - 0.9 % | T61 | AA Standards, ASTM B247 |
Mangan | 0.2 % Show Material materials with Mangan of 0.2 % | T61 | AA Standards, ASTM B247 |
Nickel | 1.7 - 2.3 % Show Material materials with Nickel of 1.7 - 2.3 % | T61 | AA Standards, ASTM B247 |
Silizium | 0.9 % Show Material materials with Silizium of 0.9 % | T61 | AA Standards, ASTM B247 |
Zink | 0.25 % Show Material materials with Zink of 0.25 % | T61 | AA Standards, ASTM B247 |
Technological properties
Property | ||
---|---|---|
Brazing | general: no brazing is known or developed | |
General machinability | General: good to acceptable | |
Workability | Moderate Workability |