Allgemein
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 2.66 g/cm³ Show Material materials with Dichte of 2.66 g/cm³ | H12 | EN 573-3, EN 1592, EN 485, EN 754 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | |
20.0 °C | 2.66 g/cm³ Show Material materials with Dichte of 2.66 g/cm³ | H12 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 573-3 | Coil, Sheet, Plate, Rod, Flat, Seamless Tube, Tube | |
20.0 °C | 2.66 - 2.67 g/cm³ Show Material materials with Dichte of 2.66 - 2.67 g/cm³ | H12 | EN 573-3 | Rod, Flat, Seamless Tube, Tube | |
20.0 °C | 2.67 g/cm³ Show Material materials with Dichte of 2.67 g/cm³ | H12 | EN 573-3 | Rod, Flat, Seamless Tube, Tube |
Abmessung
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 130.0 MPa Show Material materials with Bending Fatigue Strength of 130.0 MPa | H12 | EN 573-3, EN 1592, EN 485, EN 754 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | ||
Dehnung | 3.0 % Show Material materials with Dehnung of 3.0 % | H12 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | A50 | |
3.0 - 6.0 % Show Material materials with Dehnung of 3.0 - 6.0 % | H12 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Plate | A50 | ||
4.0 % Show Material materials with Dehnung of 4.0 % | H12 | EN 573-3, EN 485, EN 754 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | A50 | ||
5.0 % Show Material materials with Dehnung of 5.0 % | H12 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | A50 | ||
5.0 % Show Material materials with Dehnung of 5.0 % | H12 | EN 573-3, EN 754 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | A100 | ||
6.0 % Show Material materials with Dehnung of 6.0 % | H12 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | A50 | ||
6.0 % Show Material materials with Dehnung of 6.0 % | H12 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | A100 | ||
7.0 % Show Material materials with Dehnung of 7.0 % | H12 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | A50 | ||
9.0 % Show Material materials with Dehnung of 9.0 % | H12 | EN 573-3, EN 1592 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | A100 | ||
20.0 °C | 3.0 % Show Material materials with Dehnung of 3.0 % | H12 | EN 573-3 | Flat | A50 | |
20.0 °C | 3.0 % Show Material materials with Dehnung of 3.0 % | H12 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 4.0 % Show Material materials with Dehnung of 4.0 % | H12 | EN 573-3 | Rod, Tube, Flat | A50 | |
20.0 °C | 4.0 % Show Material materials with Dehnung of 4.0 % | H12 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 5.0 % Show Material materials with Dehnung of 5.0 % | H12 | EN 573-3 | Flat | A50 | |
20.0 °C | 5.0 % Show Material materials with Dehnung of 5.0 % | H12 | EN 573-3 | Rod, Tube | ||
20.0 °C | 5.0 % Show Material materials with Dehnung of 5.0 % | H12 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 6.0 % Show Material materials with Dehnung of 6.0 % | H12 | EN 573-3 | Flat | A50 | |
20.0 °C | 6.0 % Show Material materials with Dehnung of 6.0 % | H12 | EN 573-3 | Flat | ||
20.0 °C | 6.0 % Show Material materials with Dehnung of 6.0 % | H12 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 6.0 % Show Material materials with Dehnung of 6.0 % | H12 | EN 573-3 | Flat | Transverse | |
20.0 °C | 7.0 % Show Material materials with Dehnung of 7.0 % | H12 | EN 573-3 | Flat | A50 | |
20.0 °C | 7.0 % Show Material materials with Dehnung of 7.0 % | H12 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 9.0 % Show Material materials with Dehnung of 9.0 % | H12 | EN 573-3 | Seamless Tube | ||
Elastizitätsmodul | 71.0 GPa Show Material materials with Elastizitätsmodul of 71.0 GPa | H12 | EN 573-3, EN 1592, EN 485, EN 754 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | ||
20.0 °C | 71.0 GPa Show Material materials with Elastizitätsmodul of 71.0 GPa | H12 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 573-3 | Coil, Sheet, Plate, Rod, Flat, Seamless Tube, Tube | ||
Härte, Brinell | 81.0 [-] Show Material materials with Härte, Brinell of 81.0 [-] | H12 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | ||
20.0 °C | 81.0 [-] Show Material materials with Härte, Brinell of 81.0 [-] | H12 | EN 573-3 | Flat | ||
20.0 °C | 85.0 [-] Show Material materials with Härte, Brinell of 85.0 [-] | H12 | EN 573-3 | Rod, Tube | ||
Härte, HBW | 81 [-] Show Material materials with Härte, HBW of 81 [-] | H12 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Plate | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||||
Poissonzahl | 20.0 °C | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | H12 | EN 573-3 | Rod, Flat, Seamless Tube, Tube | |
Schubmodule | 26.7 GPa Show Material materials with Schubmodule of 26.7 GPa | H12 | EN 573-3, EN 1592, EN 485, EN 754 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | ||
27.0 GPa Show Material materials with Schubmodule of 27.0 GPa | H12 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Plate | |||
20.0 °C | 26.7 - 27.0 GPa Show Material materials with Schubmodule of 26.7 - 27.0 GPa | H12 | EN 573-3 | Rod, Flat, Seamless Tube, Tube | ||
20.0 °C | 26.7 GPa Show Material materials with Schubmodule of 26.7 GPa | H12 | EN 573-3 | Rod, Flat, Seamless Tube, Tube | ||
Streckgrenze | 170.0 MPa Show Material materials with Streckgrenze of 170.0 MPa | H12 | EN 573-3, EN 1592 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | RP02 | |
190.0 MPa Show Material materials with Streckgrenze of 190.0 MPa | H12 | EN 573-3, EN 754 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | RP02 | ||
200.0 MPa Show Material materials with Streckgrenze of 200.0 MPa | H12 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | RP02 | ||
200 MPa Show Material materials with Streckgrenze of 200 MPa | H12 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Plate | |||
20.0 °C | 170.0 MPa Show Material materials with Streckgrenze of 170.0 MPa | H12 | EN 573-3 | Seamless Tube | RP02 | |
20.0 °C | 190.0 MPa Show Material materials with Streckgrenze of 190.0 MPa | H12 | EN 573-3 | Rod, Tube | RP02 | |
20.0 °C | 200.0 MPa Show Material materials with Streckgrenze of 200.0 MPa | H12 | EN 573-3 | Flat | RP02 | |
20.0 °C | 200.0 MPa Show Material materials with Streckgrenze of 200.0 MPa | H12 | EN 573-3 | Flat | RP02 Transverse | |
Zugfestigkeit | 270.0 MPa Show Material materials with Zugfestigkeit of 270.0 MPa | H12 | EN 573-3, EN 1592, EN 754 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | ||
20.0 °C | 270.0 MPa Show Material materials with Zugfestigkeit of 270.0 MPa | H12 | EN 573-3 | Rod, Seamless Tube, Tube | ||
20.0 °C | 275.0 - 335.0 MPa Show Material materials with Zugfestigkeit of 275.0 - 335.0 MPa | H12 | EN 573-3, EN 485, EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Flat, Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire, Coil, Sheet, Plate | ||
20.0 °C | 275.0 - 335.0 MPa Show Material materials with Zugfestigkeit of 275.0 - 335.0 MPa | H12 | EN 573-3 | Flat | Transverse |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | -50 °C | 2.2e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.2e-05 1/K | H12 | EN 573-3, EN 1592, EN 485, EN 754 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire, Flat, Seamless Tube | |
-50.0 °C | 2.2e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.2e-05 1/K | H12 | EN 573-3, EN 1592, EN 485, EN 754 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire, Flat, Seamless Tube | ||
20 °C | 2.2e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.2e-05 1/K | H12 | EN 573-3, EN 1592, EN 485, EN 754 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire, Flat, Seamless Tube | ||
20 °C | 2.38e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.38e-05 1/K | H12 | EN 573-3, EN 1592, EN 485, EN 754 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire, Flat, Seamless Tube | ||
20 °C | 2.4699999999999997e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.4699999999999997e-05 1/K | H12 | EN 573-3, EN 1592, EN 485, EN 754 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | ||
20 °C | 2.58e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.58e-05 1/K | H12 | EN 573-3, EN 1592, EN 485, EN 754 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire, Flat, Seamless Tube | ||
100 °C | 2.38e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.38e-05 1/K | H12 | EN 573-3, EN 1592, EN 485, EN 754 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire, Flat, Seamless Tube | ||
100.0 °C | 2.38e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.38e-05 1/K | H12 | EN 573-3, EN 1592, EN 485, EN 754 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire, Flat, Seamless Tube | ||
100 °C | 0.000024 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 0.000024 1/K | H12 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Plate | 20-100°C | |
200 °C | 2.4699999999999997e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.4699999999999997e-05 1/K | H12 | EN 573-3, EN 1592, EN 485, EN 754 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | ||
200.0 °C | 2.47e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.47e-05 1/K | H12 | EN 573-3 | Rod, Flat, Seamless Tube, Tube | ||
300 °C | 2.58e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.58e-05 1/K | H12 | EN 573-3, EN 1592, EN 485, EN 754 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire, Flat, Seamless Tube | ||
300.0 °C | 2.58e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.58e-05 1/K | H12 | EN 573-3, EN 1592, EN 485, EN 754 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire, Flat, Seamless Tube | ||
Max. Betriebstemperatur | 150.0 °C Show Material materials with Max. Betriebstemperatur of 150.0 °C | Typical for Wrought 5000 Series Aluminium | ||||
Schmelzpunkt | 585.0 - 641.0 °C Show Material materials with Schmelzpunkt of 585.0 - 641.0 °C | H12 | EN 573-3, EN 1592, EN 485, EN 754 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | ||
585.0 - 640.0 °C Show Material materials with Schmelzpunkt of 585.0 - 640.0 °C | H12 | EN 573-3, EN 1592, EN 485, EN 754 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | |||
Spezifische Wärmekapazität | 900.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 900.0 J/(kg·K) | H12 | EN 573-3, EN 1592, EN 485, EN 754 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | ||
20.0 °C | 900.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 900.0 J/(kg·K) | H12 | EN 573-3 | Rod, Flat, Seamless Tube, Tube | ||
Wärmeleitfähigkeit | 126 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 126 W/(m·K) | H12 | EN 573-3, EN 1592, EN 485, EN 754, EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire, Coil, Sheet, Plate | ||
20.0 °C | 120.0 - 140.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 120.0 - 140.0 W/(m·K) | H12 | EN 573-3, EN 1592, EN 485, EN 754 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire, Flat, Seamless Tube | ||
20.0 °C | 120.0 - 126.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 120.0 - 126.0 W/(m·K) | H12 | EN 573-3 | Rod, Flat, Seamless Tube, Tube | ||
20.0 °C | 126.0 - 140.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 126.0 - 140.0 W/(m·K) | H12 | EN 573-3 | Rod, Flat, Seamless Tube, Tube | ||
20.0 °C | 126.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 126.0 W/(m·K) | H12 | EN 573-3 | Rod, Flat, Seamless Tube, Tube |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Elektrische Leitfähigkeit | 18000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 18000000.0 S/m | H12 | EN 573-3, EN 1592, EN 485, EN 754 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | |
20.0 °C | 17000000.0 - 19000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 17000000.0 - 19000000.0 S/m | H12 | EN 573-3, EN 1592, EN 485, EN 754 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire, Flat, Seamless Tube | |
spezifischer Widerstand | 5.26e-08 - 5.88e-08 Ω·m Show Material materials with spezifischer Widerstand of 5.26e-08 - 5.88e-08 Ω·m | H12 | EN 573-3, EN 1592, EN 485, EN 754 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | |
5.56e-08 Ω·m Show Material materials with spezifischer Widerstand of 5.56e-08 Ω·m | H12 | EN 573-3, EN 1592, EN 485, EN 754 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | ||
20.0 °C | 5.2e-08 - 5.6e-08 Ω·m Show Material materials with spezifischer Widerstand of 5.2e-08 - 5.6e-08 Ω·m | H12 | EN 573-3 | Rod, Flat, Seamless Tube, Tube | |
20.0 °C | 5.2e-08 - 5.8e-08 Ω·m Show Material materials with spezifischer Widerstand of 5.2e-08 - 5.8e-08 Ω·m | H12 | EN 573-3 | Rod, Flat, Seamless Tube, Tube | |
20.0 °C | 5.6e-08 Ω·m Show Material materials with spezifischer Widerstand of 5.6e-08 Ω·m | H12 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 573-3 | Coil, Sheet, Plate, Rod, Flat, Seamless Tube, Tube | |
20.0 °C | 5.6e-08 - 5.8e-08 Ω·m Show Material materials with spezifischer Widerstand of 5.6e-08 - 5.8e-08 Ω·m | H12 | EN 573-3 | Rod, Flat, Seamless Tube, Tube |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Andere | 0.05 - 0.15 % Show Material materials with Andere of 0.05 - 0.15 % | H12 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Plate |
Chrom | 0.05 - 0.25 % Show Material materials with Chrom of 0.05 - 0.25 % | H12 | EN 573-3, EN 1592, EN 485, EN 754, EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Rod, Flat, Seamless Tube, Tube, Strip, Sheet, Plate, Welded Tube, Wire, Coil, Sheet, Plate |
Eisen | 0.5 % Show Material materials with Eisen of 0.5 % | H12 | EN 573-3 | Rod, Flat, Seamless Tube, Tube |
0.50 % Show Material materials with Eisen of 0.50 % | H12 | EN 573-3, EN 1592, EN 485, EN 754 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | |
0.5 % Show Material materials with Eisen of 0.5 % | H12 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Plate | |
Kupfer | 0.1 % Show Material materials with Kupfer of 0.1 % | H12 | EN 573-3, EN 1592, EN 485, EN 754 | Rod, Flat, Seamless Tube, Tube, Strip, Sheet, Plate, Welded Tube, Wire |
0.1 % Show Material materials with Kupfer of 0.1 % | H12 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Plate | |
Magnesium | 3.5 - 4.5 % Show Material materials with Magnesium of 3.5 - 4.5 % | H12 | EN 573-3, EN 1592, EN 485, EN 754, EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Rod, Flat, Seamless Tube, Tube, Strip, Sheet, Plate, Welded Tube, Wire, Coil, Sheet, Plate |
Mangan | 0.2 - 0.7 % Show Material materials with Mangan of 0.2 - 0.7 % | H12 | EN 573-3, EN 1592, EN 485, EN 754, EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Rod, Flat, Seamless Tube, Tube, Strip, Sheet, Plate, Welded Tube, Wire, Coil, Sheet, Plate |
Silizium | 0.4 % Show Material materials with Silizium of 0.4 % | H12 | EN 573-3, EN 1592, EN 485, EN 754 | Rod, Flat, Seamless Tube, Tube, Strip, Sheet, Plate, Welded Tube, Wire |
0.4 % Show Material materials with Silizium of 0.4 % | H12 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Plate | |
Titan | 0.15 % Show Material materials with Titan of 0.15 % | H12 | EN 573-3, EN 1592, EN 485, EN 754 | Rod, Flat, Seamless Tube, Tube, Strip, Sheet, Plate, Welded Tube, Wire |
0.15 % Show Material materials with Titan of 0.15 % | H12 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Plate | |
Zink | 0.25 % Show Material materials with Zink of 0.25 % | H12 | EN 573-3, EN 1592, EN 485, EN 754 | Rod, Flat, Seamless Tube, Tube, Strip, Sheet, Plate, Welded Tube, Wire |
0.25 % Show Material materials with Zink of 0.25 % | H12 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Plate |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: acceptable, Protective: very good | |
Application areas | Vessels: Pressure, Cryogenics; Components: Access hatches, Spoilers, General tranportation | |
Brazing | hard brazing (with flux/ without flux): poor / sufficient, friction soldering: acceptable, soft brazing with flux: poor | |
Corrosion properties | Excellent | |
Welding | Good | |
Workability | Bending / Spinning (cold): good / sufficient, Impact extrusion (cold): sufficient, Deep drawing / upsetting (Condition) good (O) / good (O) |