Allgemein
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 60.0 - 90.0 MPa Show Material materials with Bending Fatigue Strength of 60.0 - 90.0 MPa | F | EN 1706, EN 13195 | Casting | ||
Elastizitätsmodul | 68.0 GPa Show Material materials with Elastizitätsmodul of 68.0 GPa | F | EN 1706, EN 13195 | Casting | ||
20.0 °C | 68.0 GPa Show Material materials with Elastizitätsmodul of 68.0 GPa | F | EN 1706 | |||
Härte, Brinell | 70.0 [-] Show Material materials with Härte, Brinell of 70.0 [-] | F | EN 1706, EN 13195 | Casting | ||
20.0 °C | 70.0 [-] Show Material materials with Härte, Brinell of 70.0 [-] | F | EN 1706 | |||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Cast 5xx.x Series Aluminium | ||||
Zugfestigkeit | 200.0 MPa Show Material materials with Zugfestigkeit of 200.0 MPa | F | EN 1706, EN 13195 | Casting | ||
20.0 °C | 200.0 MPa Show Material materials with Zugfestigkeit of 200.0 MPa | F | EN 1706 |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 20 °C | 2.4e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.4e-05 1/K | F | EN 1706, EN 13195 | Casting |
20 °C | 2.4999999999999998e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.4999999999999998e-05 1/K | F | EN 1706, EN 13195 | Casting | |
100.0 °C | 2.4e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.4e-05 1/K | F | EN 1706, EN 13195 | Casting | |
100 °C | 2.4e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.4e-05 1/K | F | EN 1706, EN 13195 | Casting | |
200 °C | 2.4999999999999998e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.4999999999999998e-05 1/K | F | EN 1706, EN 13195 | Casting | |
Schmelzpunkt | 530.0 - 620.0 °C Show Material materials with Schmelzpunkt of 530.0 - 620.0 °C | F | EN 1706, EN 13195 | Casting | |
Spezifische Wärmekapazität | 940.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 940.0 J/(kg·K) | F | EN 1706, EN 13195 | Casting | |
20.0 °C | 940.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 940.0 J/(kg·K) | F | EN 1706 | ||
Wärmeleitfähigkeit | 20.0 °C | 60.0 - 90.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 60.0 - 90.0 W/(m·K) | F | EN 1706, EN 13195 | Casting |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Elektrische Leitfähigkeit | 20.0 °C | 11000000.0 - 14000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 11000000.0 - 14000000.0 S/m | F | EN 1706, EN 13195 | Casting |
spezifischer Widerstand | 7.14e-08 - 9.09e-08 Ω·m Show Material materials with spezifischer Widerstand of 7.14e-08 - 9.09e-08 Ω·m | F | EN 1706, EN 13195 | Casting |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminium | 84.45 % Show Material materials with Aluminium of 84.45 % | F | EN 1706 | |
Blei | 0.1 % Show Material materials with Blei of 0.1 % | F | EN 1706, EN 13195 | Casting |
Eisen | 1.0 % Show Material materials with Eisen of 1.0 % | F | EN 1706 | |
1.00 % Show Material materials with Eisen of 1.00 % | F | EN 1706, EN 13195 | Casting | |
Kupfer | 0.1 % Show Material materials with Kupfer of 0.1 % | F | EN 1706, EN 13195 | Casting |
Magnesium | 8.0 - 10.5 % Show Material materials with Magnesium of 8.0 - 10.5 % | F | EN 1706, EN 13195 | Casting |
Mangan | 0.55 % Show Material materials with Mangan of 0.55 % | F | EN 1706, EN 13195 | Casting |
Nickel | 0.1 % Show Material materials with Nickel of 0.1 % | F | EN 1706, EN 13195 | Casting |
Silizium | 2.5 % Show Material materials with Silizium of 2.5 % | F | EN 1706, EN 13195 | Casting |
Titan | 0.2 % Show Material materials with Titan of 0.2 % | F | EN 1706, EN 13195 | Casting |
Zink | 0.25 % Show Material materials with Zink of 0.25 % | F | EN 1706, EN 13195 | Casting |
Zinn | 0.1 % Show Material materials with Zinn of 0.1 % | F | EN 1706, EN 13195 | Casting |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: good | |
Corrosion properties | general: excellent | |
General machinability | after thermal treatment: excellent | |
Processing methods | pressure die casting, separately cast test sample |